A technology of water-soluble acrylic and high alcohol resistance, applied in the direction of coating, etc., can solve the problems of poor alcohol resistance, achieve the effect of improving alcohol resistance, reducing the influence of alcohol solvent, and increasing the effect of alcohol resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] A high alcohol-resistant water-soluble acrylic resin, comprising the following components by weight: 5 parts of lauryl methacrylate, 10 parts of methyl methacrylate, 5 parts of butyl acrylate, 20 parts of styrene, acrylonitrile 5 parts, 5 parts of methacrylic acid, 9 parts of butyl methacrylate, 1 part of initiator (tert-butyl peroxybenzoate), 25 parts of propylene glycol methyl ether and 15 parts of industrial ethanol.
[0024] The preparation method of above-mentioned high alcohol-resistant water-soluble acrylic resin comprises the steps:
[0025] (1) Under the protection of inert gas, put 25 parts of propylene glycol methyl ether into the reaction kettle, then raise the temperature to 120°C, and maintain this temperature after heating;
[0026] (2) 10 parts of methyl methacrylate, 5 parts of butyl acrylate, 20 parts of styrene, 5 parts of dodecyl methacrylate, 5 parts of acrylonitrile, 9 parts of methacrylic acid Put butyl ester, 5 parts of methacrylic acid and 0.8 ...
Embodiment 2
[0029] A high alcohol-resistant water-soluble acrylic resin, comprising the following components by weight: 3 parts of lauryl methacrylate, 8 parts of methyl methacrylate, 4 parts of butyl acrylate, 18 parts of styrene, acrylonitrile 7 parts, 5 parts of methacrylic acid, 14 parts of butyl methacrylate, 2 parts of initiator (tert-butyl peroxybenzoate), 30 parts of propylene glycol methyl ether and 10 parts of industrial ethanol.
[0030] The preparation method of above-mentioned high alcohol-resistant water-soluble acrylic resin comprises the steps:
[0031] (1) Under the protection of inert gas, put 30 parts of propylene glycol methyl ether into the reaction kettle, then raise the temperature to 118°C, and maintain this temperature after heating;
[0032] (2) 8 parts of methyl methacrylate, 4 parts of butyl acrylate, 18 parts of styrene, 3 parts of dodecyl methacrylate, 7 parts of acrylonitrile, 14 parts of methacrylic acid Put butyl ester, 5 parts of methacrylic acid and 1.5...
Embodiment 3
[0035] A high alcohol-resistant water-soluble acrylic resin, comprising the following components by weight: 4 parts of lauryl methacrylate, 12 parts of methyl methacrylate, 8 parts of butyl acrylate, 17 parts of styrene, acrylonitrile 3 parts, 8 parts of methacrylic acid, 10 parts of butyl methacrylate, 1.5 parts of initiator (tert-butyl peroxybenzoate), 28 parts of propylene glycol methyl ether and 12 parts of industrial ethanol.
[0036] The preparation method of above-mentioned high alcohol-resistant water-soluble acrylic resin comprises the steps:
[0037] (1) Under the protection of an inert gas, put 28 parts of propylene glycol methyl ether into the reaction kettle, then heat up to 122°C, and maintain this temperature after heating;
[0038](2) 12 parts of methyl methacrylate, 8 parts of butyl acrylate, 17 parts of styrene, 4 parts of dodecyl methacrylate, 3 parts of acrylonitrile, 10 parts of methacrylic acid Put butyl ester, 8 parts of methacrylic acid and 1.2 parts o...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com