Asphalt pavement seal material as well as preparation method and application thereof

A technology of asphalt pavement and hard asphalt, which is applied in the field of asphalt pavement sealant and its preparation, can solve the problems of insufficient durability, weak water sealing performance, and low cohesive force, so as to prevent the decline of anti-skid performance and excellent anti-skid performance. Abrasion and water repellency, improve the effect of friction

Active Publication Date: 2022-05-03
CHINA PETROLEUM & CHEM CORP
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, currently used asphalt pavement maintenance materials such as micro-surfacing and slurry seals usually have poor wear resistance, low cohesive force, weak water sealing performance, and the durability is not good enough

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Asphalt pavement seal material as well as preparation method and application thereof
  • Asphalt pavement seal material as well as preparation method and application thereof
  • Asphalt pavement seal material as well as preparation method and application thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0091] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:

[0092] High aromatics oil: 30 grams, extracted oil from vacuum side stream furfural refined by Maoming Petrochemical, aromatics content 77%;

[0093] High colloidal oil: 10 grams, heavy deasphalted oil produced by Maoming Petrochemical Co., Ltd., with a colloid content of 24.3%;

[0094] Rubber powder modifier: 5 grams, waste rubber powder produced by Lefeng Recycling Materials Company, fineness 60 mesh;

[0095] Hard asphalt: 5 grams, petroleum asphalt produced by Maoming Petrochemical, penetration 29 (0.1mm);

[0096] Plasticizer: 2 grams, the epoxidized soybean oil produced by Zhenxing Chemical Company;

[0097] Adhesion enhancer: 3 grams, bisphenol A type epoxy resin produced by Zhujiang Chemical Coatings Company;

[0098] Thinner: 25 grams, solvent gasoline produced by Maoming Petrochemical, impurity content <0.2%...

Embodiment 2

[0107] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:

[0108] High aromatics oil: 70 grams, extracted oil from vacuum side stream furfural refined by Maoming Petrochemical, aromatics content 69%;

[0109] High colloidal oil: 20 grams, heavy deasphalted oil produced by Maoming Petrochemical Co., Ltd., with a colloid content of 17.1%;

[0110] Rubber powder modifier: 10 grams, waste rubber powder produced by Lingzhong Composite Materials Company, fineness 80 mesh;

[0111] Hard asphalt: 10 grams, petroleum asphalt produced by Maoming Petrochemical, penetration 22 (0.1mm);

[0112] Plasticizer: 4 grams, the epoxidized soybean oil produced by Zhenxing Chemical Company;

[0113]Bonding enhancer: 6 grams, bisphenol A type epoxy resin produced by Nanke New Material Chemical Company;

[0114] Thinner: 40 grams, solvent gasoline produced by Maoming Petrochemical, impurity content <...

Embodiment 3

[0123] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:

[0124] High aromatics oil: 40 grams, extracted oil from vacuum side stream furfural refined by Maoming Petrochemical, aromatics content 77%;

[0125] High colloidal oil: 12 grams, heavy deasphalted oil produced by Maoming Petrochemical Co., Ltd., with a colloid content of 15.4%;

[0126] Rubber powder modifier: 6 grams, waste rubber powder produced by Lingzhong Composite Materials Company, fineness 80 mesh;

[0127] Hard asphalt: 6 grams, petroleum asphalt produced by Maoming Petrochemical, penetration 26 (0.1mm);

[0128] Plasticizer: 2.5 grams, the epoxidized soybean oil produced by Zhongmao Gaoke Chemical Company;

[0129] Bonding enhancer: 3.5 grams, bisphenol A type epoxy resin produced by Nanke New Material Chemical Company;

[0130] Thinner: 30 grams, solvent gasoline produced by Maoming Petrochemical, impurity ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Finenessaaaaaaaaaa
Maximum particle sizeaaaaaaaaaa
Maximum particle sizeaaaaaaaaaa
Login to View More

Abstract

The invention relates to an asphalt pavement seal material as well as a preparation method and application thereof. The seal material comprises high aromatic oil, high gummy oil, a rubber powder modifier, hard asphalt, a plasticizer, a bonding enhancer, a diluent and aggregate. The asphalt pavement maintenance agent can be applied to preventive maintenance of asphalt pavements, is convenient and quick to construct, can form a super-strong protection layer on the asphalt pavements after being used, prevents water and air from entering the asphalt pavements to cause damage to pavement structures, and has a sealing and healing effect on fine cracks of the asphalt pavements. In addition, the asphalt pavement anti-skid agent also has excellent anti-wear and waterproof capabilities, not only can improve the friction force of an asphalt pavement and prevent the anti-skid performance of the pavement from being reduced, but also can protect and repair a binding material lost due to aging on the surface of the asphalt pavement, effectively prevent water from permeating and eroding the internal structure of the pavement, and prolong the service life of the asphalt pavement.

Description

technical field [0001] The invention belongs to the technical field of oil refining and chemical materials, and in particular relates to an asphalt pavement sealing material and its preparation method and application. Background technique [0002] Due to its good performance such as comfortable driving, low noise, and smooth road surface, asphalt roads are more and more used in all levels of roads in our country, especially in our country's expressways, which basically use asphalt roads. However, after the asphalt road is used for a period of time, due to the repeated friction and rolling of the traffic load, natural sunlight, and rain erosion, certain diseases will gradually occur on the road surface. The longer the use time, the deeper the degree of disease. In order to ensure the normal use of asphalt roads, it is usually necessary to implement corresponding preventive maintenance treatments on the asphalt pavement after a certain period of use, so as to prevent road surf...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C04B26/26C04B111/20
CPCC04B26/26C04B2111/0075C04B2111/2038C04B2111/00293C04B24/36C04B18/22C04B24/08C04B24/281C04B14/14C04B14/06
Inventor 何靖斌罗辉洪黄艳芳欧晔苏亦平梁红梅
Owner CHINA PETROLEUM & CHEM CORP