Beneficiation reagent for lead flotation of lead-zinc flotation and preparation method of beneficiation reagent
A lead-zinc and flotation technology, used in flotation, solid separation, etc., can solve the problem of large amount of lime, achieve the effect of small amount of lime, reduce zinc content, and improve quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] The lead-zinc flotation method of the ore comprises the following steps:
[0023] a. The crushed lead-zinc-silver ore is ground, and the zinc sulfate is put into the grinding process; the amount of zinc sulfate added is 1000 grams per ton of ore; the grinding process is divided into two stages for grinding, and the first stage adopts a grid ball mill Grind the ore to 200 mesh and the ore powder accounts for 50%, and add zinc sulfate in the first stage of grinding; the second stage uses overflow ball milling equipment to continue grinding the powder after the first stage to 200 mesh Grinding products with mineral powder accounting for more than 76%;
[0024] b, put the ground ore in step a into the mixing drum, and add slaked lime and sodium sulfite in the mixing drum to fully stir; wherein, the addition of sodium sulfite is 150 grams per ton of ore; the addition of slaked lime is 1200 grams per ton tons of ore; adjust the pH of the pulp to 9;
[0025] c, in the materi...
Embodiment 2
[0029] The lead-zinc flotation method of the ore comprises the following steps:
[0030] a. The crushed lead-zinc-silver ore is ground, and the zinc sulfate is put into the grinding process; the amount of zinc sulfate added is 800 grams per ton of ore; the grinding process is divided into two stages for grinding, and the first stage adopts a grid ball mill Grind the ore to 200 mesh and the ore powder accounts for 50%, and add zinc sulfate in the first stage of grinding; the second stage uses overflow ball milling equipment to continue grinding the powder after the first stage to 200 mesh Grinding products with mineral powder accounting for more than 76%;
[0031] b. Put the ground ore in the step a into the mixing drum, and add slaked lime and sodium sulfite in the mixing drum to fully stir; wherein, the addition of sodium sulfite is 100 grams per ton of ore; the addition of slaked lime is 1000 grams per ton tons of ore; adjust the pH of the pulp to 9;
[0032] c, in the mat...
Embodiment 3
[0036] The lead-zinc flotation method of the ore comprises the following steps:
[0037] a. The crushed lead, zinc and silver raw ore is ground and processed, and the zinc sulfate is put into the grinding process; the addition amount of zinc sulfate is 900 grams per ton of ore; the grinding process is divided into two stages for grinding, and the first stage adopts a grid-type ball mill Grind the ore to 200 mesh and the ore powder accounts for 50%, and add zinc sulfate in the first stage of grinding; the second stage uses overflow ball milling equipment to continue grinding the powder after the first stage to 200 mesh Grinding products with mineral powder accounting for more than 76%;
[0038] b, put the ore ground in step a into the mixing drum, and add slaked lime and sodium sulfite in the mixing drum to fully stir; wherein, the addition of sodium sulfite is 125 grams per ton of ore; the addition of slaked lime is 1100 grams per ton tons of ore; adjust the pH of the pulp to...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com