Leather glue prepared by adopting waste materials and preparation method thereof

A waste rubber and waste technology, applied in the field of leather glue and its preparation, can solve the problems of non-natural degradation, pollution, non-rotten transformation, etc., and achieve the effects of saving raw materials, high bonding strength, and good water resistance

Inactive Publication Date: 2009-11-18
北京道顺国际技术开发有限责任公司
View PDF0 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] At present, there are various formulations of cavity adhesives, and the performance of the adhesives varies greatly according to their respective components. However, most adhesives, such as phenolic resin adhesives, contain harmful substances such as benzene, toluene, xylene, and formaldehyde. Use Not only may it cause serious pollution indoors, but it will become an important source of harmful substances such as formaldehyde, which will damage people's health. In addition, the manufacturing process of these adhesives is relatively complicated and the cost is relatively high.
[0003] On the other hand, the amount of polystyrene foam plastics and rubber products in my country is increasing, and most of them are for one-time use. Millions of tons of white garbage and waste rubber products are scattered in nature and cannot be decomposed and transformed. It cannot be degraded naturally, causing serious pollution. The current treatment methods for these pollutants are generally incineration and landfill. Among them, landfill will occupy a large amount of land, and incineration will cause new air pollution problems.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0023] Adhesive composition ratio:

[0024] Special base glue mother liquor: 55 parts;

[0025] Special silicone coupling agent: 6 parts;

[0026] Natural latex: 10 parts;

[0027] Polyacrylate: 3 parts;

[0028] Sodium isobutyl naphthalene sulfonate: 0.5 part;

[0029] Sodium salicylate: 0.5 parts;

[0030] Sodium methyl dinaphthalene sulfonate: 1 part;

[0031] Zinc oxide: 1.5 parts;

[0032] Calcium carbonate: 6 servings.

[0033] Among them, the special base glue mother liquor (base) components are as follows:

[0034] Waste rubber tires: 10 parts;

[0035] Waste polystyrene: 35 parts;

[0036] Solvent naphtha 200#: 70 parts.

[0037] Preparation:

[0038] (1) Prepare special base material glue mother liquor: decontaminate waste rubber tires and waste polystyrene, wash and dry, then send them to a closed-type powerful pulverizer for crushing, and put them into a semi-closed container in proportion to solvent liquid oil Stir evenly at room temperature to make a ...

Embodiment 2

[0041] Adhesive composition ratio:

[0042] Special base glue mother liquor: 45 parts;

[0043] Special silicone coupling agent: 10 parts;

[0044] Natural latex: 15 parts;

[0045] Polyacrylate: 1.5 parts;

[0046] Sodium isobutyl naphthalene sulfonate: 1 part

[0047] Sodium salicylate: 1 part;

[0048] Sodium methyl dinaphthalene sulfonate: 0.5 parts;

[0049] Zinc oxide: 3 parts;

[0050] Calcium Carbonate: 1 part.

[0051] Among them, the special base glue mother liquor (base) components are as follows:

[0052] Waste rubber tires: 25 parts;

[0053] Waste polystyrene: 30 parts;

[0054] Solvent naphtha 200#: 60 parts.

[0055] The preparation method is the same as in Example 1.

Embodiment 3

[0057] Adhesive composition ratio:

[0058] Special base glue mother liquor: 50 parts;

[0059] Special silicone coupling agent: 8 parts;

[0060] Natural latex: 13 parts;

[0061] Polyacrylate: 2 parts;

[0062] Sodium isobutyl naphthalene sulfonate: 0.8 parts;

[0063] Sodium salicylate: 0.8 parts;

[0064] Sodium methyl dinaphthalene sulfonate: 0.8 parts;

[0065] Zinc oxide: 2.3 parts;

[0066] Calcium Carbonate: 4 parts.

[0067] Among them, the special base glue mother liquor (base) components are as follows:

[0068] Waste rubber tires: 18 parts;

[0069] Waste polystyrene: 32 parts;

[0070] Solvent naphtha 200#: 80 parts.

[0071] The preparation method is the same as in Example 1.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to leather glue prepared by adopting waste materials and a preparation method thereof. The glue comprises raw materials of 45-55 portions of special base glue mother liquid, 6-10 portions of special organosilicone coupling agent, 10-15 portions of natural emulsion, 1.5-3 portions of salt polyacrylate, 0.5-1 portion of dinaphthyl sodium sulfonate, 0.5-1 portion of sodium salicylate, 0.5-1 portion of methyl dinaphthyl sodium sulfonate, 1.5-3 portions of zinc oxide and 1-6 portions of calcium carbonate, wherein the special base glue mother liquid is prepared by adopting No.200 solvent naphtha to dissolve waste polystyrene and waste rubber tires, and the special organosilicone coupling agent is obtained in such a way that asphaltum and waste glass react in a high-temperature reactor. The raw materials are put in a retort and are evenly stirred at the temperature of 65-100 DEG C so as to be processed by polymerization for 2 hours, and a binder of the invention is obtained after cooling the product of reaction. The invention adopts waste plastic and rubber as raw materials, thereby being beneficial to reducing environmental pollution, saving material resources, having low production cost and being suitable for the binding of various materials, in particular the binding of soft materials such as leather, and the like.

Description

technical field [0001] The invention relates to a leather glue prepared from waste materials and a preparation method thereof. Background technique [0002] At present, there are various formulations of cavity adhesives, and the performance of the adhesives varies greatly according to their respective components. However, most adhesives, such as phenolic resin adhesives, contain harmful substances such as benzene, toluene, xylene, and formaldehyde. Use In the end, not only may cause serious pollution indoors, but also become an important source of harmful substances such as formaldehyde, which will damage people's health. In addition, the manufacturing process of these adhesives is relatively complicated and the cost is relatively high. [0003] On the other hand, the amount of polystyrene foam plastics and rubber products in my country is increasing, and most of them are for one-time use. Millions of tons of white garbage and waste rubber products are scattered in nature an...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C09J187/00C09J11/06C09J107/02C09J133/02
Inventor 董志刚高原杨娜娜李伟
Owner 北京道顺国际技术开发有限责任公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products