Milky white clinker for glaze and preparation method for clinker
A milky white and frit technology, applied in the field of ceramic frit and frit, can solve the problems of poor fluidity at high temperature, affect product quality, high viscosity at high temperature, etc., and achieve the effect of high flatness, good gloss, and wide firing temperature
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A milky white frit for glaze, the parts by weight of each component are:
[0016] 5 parts of potassium feldspar, 15 parts of quartz, 15 parts of albite feldspar, 5 parts of dolomite, 1 part of light calcium, 8 parts of zinc oxide, 10 parts of zirconium silicate, 1 part of potassium carbonate, 2 parts of borax, 0.5 part of barium carbonate and 1 part of aluminum oxide.
[0017] Its preparation method comprises the following steps:
[0018] Weigh 5 parts of potassium feldspar, 15 parts of quartz, 15 parts of albite, 5 parts of dolomite, 1 part of light calcium, 8 parts of zinc oxide, 10 parts of zirconium silicate, 1 part of potassium carbonate, 2 parts of borax, barium carbonate 0.5 part and 1 part of alumina, mix and stir evenly, melt in a high-temperature frit furnace at 1500°C for 1.5 hours, quench the molten liquid with cold water, and obtain milky white frit for glaze.
Embodiment 2
[0020] A milky white frit for glaze, the parts by weight of each component are:
[0021] Potassium feldspar 15 parts, quartz 25 parts, albite feldspar 25 parts, dolomite 15 parts, light calcium 5 parts, zinc oxide 15 parts, zirconium silicate 15 parts, potassium carbonate 5 parts, borax 10 parts, barium carbonate 2 parts and 5 parts of aluminum oxide.
[0022] Its preparation method comprises the following steps:
[0023] Weigh 15 parts of potassium feldspar, 25 parts of quartz, 25 parts of albite, 15 parts of dolomite, 5 parts of light calcium, 15 parts of zinc oxide, 15 parts of zirconium silicate, 5 parts of potassium carbonate, 10 parts of borax, barium carbonate 2 parts and 5 parts of alumina, mix and stir evenly, melt in a high-temperature frit furnace at 1600°C for 2.0 hours, quench the molten liquid with cold water, and obtain milky white frit for glaze.
Embodiment 3
[0025] A milky white frit for glaze, the parts by weight of each component are:
[0026] Potassium feldspar 10 parts, quartz 20 parts, albite feldspar 20 parts, dolomite 10 parts, light calcium 2 parts, zinc oxide 10 parts, zirconium silicate 12 parts, potassium carbonate 3 parts, borax 8 parts, barium carbonate 1.5 parts and 3 parts of aluminum oxide.
[0027] Its preparation method comprises the following steps:
[0028] Weigh 10 parts of potassium feldspar, 20 parts of quartz, 20 parts of albite, 10 parts of dolomite, 2 parts of light calcium, 10 parts of zinc oxide, 12 parts of zirconium silicate, 3 parts of potassium carbonate, 8 parts of borax, barium carbonate 1.5 parts and 3 parts of alumina, mix and stir evenly, melt in a high-temperature frit furnace at 1550°C for 1.8 hours, quench the molten liquid with cold water, and obtain milky white frit for glaze.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com