A cement grinding aid and high-efficiency technology, applied in the field of high-efficiency activated cement grinding aid and its preparation, can solve the problems of poor pertinence, inability to save costs for cement enterprises, single performance of the grinding aid, etc. Save production cost, good adsorption effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0020] To prepare 100 kg of high-efficiency activated cement grinding aid, weigh 18 kg of triethanolamine, 10 kg of triisopropanolamine, 7 kg of sodium carbonate, 5 kg of ethylene glycol, 30 kg of water, 5 kg of toluene, 2 kg of silica fume, and 15 kg of black liquor and 8 kg of waste liquor from sugar factories.
[0021] Its preparation method comprises the following steps:
[0022] (1) First add silica fume to toluene, stir to dissolve it and set aside;
[0023] (2) Add triisopropanolamine to water and heat to 50°C to dissolve it quickly;
[0024] (3) Add sodium carbonate, toluene dissolved in silica fume, papermaking black liquor, sugar factory waste liquor, ethylene glycol, and triethanolamine in sequence while stirring in step (2), and finally stir evenly to obtain the finished product.
[0025] The dosage of grinding aid in this embodiment is 0.1% / ton of cement. Two samples of 5kg of cement raw material and 5g of grinding aid were weighed respectively, and tested. The...
Embodiment 2
[0033] To prepare 100 kg of high-efficiency activated cement grinding aid, weigh 20 kg of triethanolamine, 8 kg of triisopropanolamine, 10 kg of sodium carbonate, 3 kg of ethylene glycol, 30 kg of water, 8 kg of toluene, 3 kg of silica fume, and 13 kg of black liquor and 5 kg of waste liquor from sugar factories. The preparation method is the same as in Example 1.
Embodiment 3
[0035] To prepare 100 kg of high-efficiency activated cement grinding aid, weigh 15 kg of triethanolamine, 5 kg of triisopropanolamine, 10 kg of sodium carbonate, 5 kg of propylene glycol, 25 kg of water, 7 kg of toluene, 3 kg of silica fume, papermaking black liquor 20 kg, 10 kg of sugar factory waste liquid. The preparation method is the same as in Example 1.