Production method of leather for cow leather clothes

A production method and garment technology, which can be applied to leather impregnation, leather manufacturing, leather surface treatment, etc., can solve the problems of large extensibility, poor smooth and bright performance, easy deformation, etc., and achieve improved performance, improved leather grade, and reduced production costs. Effect

Inactive Publication Date: 2012-07-18
河北东明牛皮制革有限公司
View PDF5 Cites 23 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] With the continuous progress and development of society, people's living standards continue to improve, material and cultural enrichment, the demand for leather and its products in domestic and foreign markets is also increasing, and the quality is getting higher

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Example Embodiment

[0046] Example 1

[0047] Production method of cowhide clothing leather:

[0048] After the leather production is softened, squeezed and shaved, it enters the retanning process, neutralization, filling dyeing, and oiling process:

[0049] Retanning: (1) Add the shaved leather to the drum, add 300% water, and rotate for 20 minutes at 45°C;

[0050] (2) Add water 150%, oxalic acid 0.8%, emulsifier BORRON SAF 0.5%, degreasing agent DESOAGEN DN 0.5%, rotate at 55°C for 60 minutes to pH 3.5-3.7, control water and wash with water;

[0051] (3) Add 220% water and 1% sodium formate, rotate at 45°C for 15-40 minutes to a pH of 4.1-4.3; add acid softening enzyme Angentan BE1%, continue rotating for 120 minutes, control water and wash with water;

[0052] (4) Add water 80%, chromium powder 2%, chromium additives Tannesco HN liq 6%, electrolyte-resistant fatliquor Quimiderm NP-2 1.0%, rotate for 120 minutes at 45°C; add 2% fatty aldehyde, rotate for 40 minutes; Add 1.5% sodium formate, continue to ...

Example Embodiment

[0079] Example 2

[0080] Production method of cowhide clothing leather:

[0081] After the leather production is softened, squeezed and shaved, it enters the retanning process, neutralization, filling dyeing, and oiling process:

[0082] Retanning: (1) Add the shaved leather into the drum, add 150% water, and rotate for 20 minutes at 35°C;

[0083] (2) Add water 250%, oxalic acid 1%, emulsifier BORRON SAF 0.8%, degreasing agent Euspon OE 1.0%, rotate at 55°C for 80 minutes to pH 3.5-3.7, control water and wash with water;

[0084] (3) Add 150% water and 0.5% sodium formate, rotate at 35°C for 15-40 minutes to pH 4.1-4.3; add acid softening enzyme Nowolase WB 3%, continue rotating for 150 minutes, control water and wash with water;

[0085] (4) Add water 200%, chromium powder 2.5%, chromium additives Quimitan ABC liquido 6%, electrolyte-resistant fatliquor Quimisoft EM 1.0%, rotate 100 minutes at 30℃; add 3% fatty aldehyde, rotate 40 minutes; add sodium formate 1.5%, continue to rotate ...

Example Embodiment

[0112] Example 3

[0113] Production method of cowhide clothing leather:

[0114] After the leather production is softened, squeezed and shaved, it enters the retanning process, neutralization, filling dyeing, and oiling process:

[0115] Retanning: (1) Add the shaved leather to the drum, add 250% water, and rotate for 20 minutes at 55°C;

[0116] (2) Add water 300%, oxalic acid 0.5%, emulsifier BORRON SAF 0.5%, degreasing agent Baymol AN2-C 0.6%, rotate at 55°C for 120 min to pH 3.5-3.7, control water and wash with water;

[0117] (3) Add water 300%, sodium formate 0.9%, rotate at 40°C for 15-40 minutes to pH 4.1-4.3; add acid softening enzyme Novocor AX 2%, continue to rotate for 180 minutes, control water and wash with water;

[0118] (4) Add water 150%, chromium powder 3%, chromium additives Quimitan ABC liquido 5%, electrolyte-resistant fatliquor Desopon LQ-5 1.5%, rotate for 120 minutes at 40°C; add 2% fatty aldehyde, rotate for 40 minutes; Add 1.5% sodium formate, continue to rot...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention belongs to the field of leather production, and discloses leather for cow leather clothes and a production method of the leather for the cow leather clothes. The method comprises the following step of: by adjusting the working procedures of retanning, neutralizing, packed dyeing, oiling and coating, adding a dry shaving working procedure between a milling working procedure and a dedusting working procedure in a dry finishing working procedure, so that the leather for the cow leather clothes can be dryly shaved to have the thickness of 0.2-0.25mm. After the leather for the cow leather clothes is used, not only can the performances such as the softness, the fullness, the smoothness, the brightness, the extensibility, the hand feel and the disability coverage be greatly improved, but also the leather is thinner and lighter, thereby being wide in practical applicability.

Description

technical field [0001] The invention relates to a production method of garment leather, in particular to a production method of cowhide garment leather. Background technique [0002] With the continuous progress and development of society, people's living standards continue to improve, material and cultural enrichment, the demand for leather and its products in domestic and foreign markets is also increasing, and the quality is getting higher and higher. It is beautiful, fashionable, and practical. The current production of garment leather is heavy, poor in smoothness and brightness, high in extensibility, and easy to deform. Obviously, traditional products cannot fully meet the current social needs. Therefore require thinner, lighter, softer, more comfortable and good wide practical leather to adapt to market needs. Contents of the invention [0003] The invention provides a method for producing cowhide garment leather. Compared with the prior art, the produced garment l...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): C14C3/28C14C9/02C14C11/00C14B1/00
Inventor 谢胜虎王敏
Owner 河北东明牛皮制革有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products