Raw material formula and production method of bentonite for well drilling
A technology of bentonite and raw materials, applied in the direction of chemical instruments and methods, drilling compositions, etc., to achieve the effects of speeding up work, improving engineering quality, and improving efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Get 94.8 kilograms of calcium-based soils, 3 kilograms of alkali powder, 1 kilogram of carboxymethyl cellulose, and 1.2 kilograms of polyacrylamide for subsequent use; 94.8 kilograms of calcium-based soils are pulverized in a pulverizer, and are transferred to a pair of rollers for roller treatment, and then Add granular calcium-based soil into the mixer through a box feeder, add water and stir, then add 3 kg of alkali powder, 1 kg of carboxymethyl cellulose, and 1.2 kg of polyacrylamide into the mixer, and take it out and stack it after it has fully reacted One week to half a month, then dry, and finally use a ray mill to grind and sieve to get the finished product of bentonite for drilling.
[0021] After passing the inspection, the performance of each index is up to standard, as follows:
[0022] Viscometer (600r / min reading) = 34 (required ≥ 30); yield (plastic viscosity) = 4.5 (required ≤ 6); filtration loss (cm3) = 14.8 (required ≤ 16); fineness modulus = 1.3 (re...
Embodiment 2
[0024] Get 92 kilograms of calcium-based soils, 5 kilograms of alkali powder, 1.5 kilograms of carboxymethyl cellulose, and 1.5 kilograms of polyacrylamide for subsequent use; 92 kilograms of calcium-based soils are pulverized in a pulverizer, and are transferred to a double-roll machine to carry out double-roll processing, and then Add granular calcium-based soil into the mixer through a box feeder, add water and stir, then add 5 kg of alkali powder, 1.5 kg of carboxymethyl cellulose, and 1.5 kg of polyacrylamide into the mixer, and take it out and stack it after it has fully reacted One week to half a month, then dry, and finally use a ray mill to grind and sieve to get the finished product of bentonite for drilling.
[0025] After passing the inspection, the performance of each index is up to standard, as follows:
[0026] Viscometer (600r / min reading) = 38 (required ≥ 30); yield (plastic viscosity) = 5 (required ≤ 6); fluid loss (cm3) = 13.5 (required ≤ 16); fineness modul...
Embodiment 3
[0028] Get 96 kilograms of calcium-based soils, 2 kilograms of alkali powder, 1 kilogram of carboxymethyl cellulose, and 1 kilogram of polyacrylamide for subsequent use; 96 kilograms of calcium-based soils are pulverized in a pulverizer, and are transferred to a pair of rollers for roller treatment, and then Add granular calcium-based soil into the mixer through a box feeder, add water and stir, then add 2 kg of alkali powder, 1 kg of carboxymethyl cellulose, and 1 kg of polyacrylamide into the mixer, and take it out and stack it after it has fully reacted One week to half a month, then dry, and finally use a ray mill to grind and sieve to get the finished product of bentonite for drilling.
[0029] After passing the inspection, the performance of each index is up to standard, as follows:
[0030] Viscometer (600r / min reading) = 32 (required ≥ 30); yield (plastic viscosity) = 4.5 (required ≤ 6); fluid loss (cm3) = 15.2 (required ≤ 16); fineness modulus = 2.1 (required ≤ 2.5);...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com