An anti-cracking and middle-layer technology, applied in the direction of coating, etc., can solve the problems of not having anti-cracking and waterproof functions, poor anti-cracking and waterproof functions, and affecting the coating effect of coatings, etc., so as to solve the problem of wall cracking and good waterproof performance , The effect of simple construction process

Inactive Publication Date: 2016-05-11
黄明杰
View PDF3 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] At present, in construction and painting engineering, intermediate paint is commonly used. Although it can meet the general requirements of use, it does not have the functions of anti-cracking and waterproofing.
For example, the wall of a building has just been painted, and not long after, the wall cracks and the wall leaks, which seriously affects the paint coating effect.
[0003] With the vigorous development of the construction and painting industry, the preparation method of the original intermediate paint is slow, the construction period is long, the anti-cracking and waterproof functions are poor, and the cost is high

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Preparation method of anti-cracking waterproof middle paint and products thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0058] Embodiment 1: a kind of anti-cracking waterproof middle paint preparation method provided by the present embodiment, it comprises the following steps:

[0059] (1) Prepare raw materials, the components and weight percentages of the raw materials are as follows:

[0060] The first part of water is 5-8%,

[0061] Cellulose 0.2-0.4%,

[0062] Ethylene glycol 1.5-2.5%,

[0063] AMP-950.1-0.2%,

[0064] Dispersant 0.15-0.3%,

[0065] The first defoamer 0.2-0.4%,

[0066] Preservatives 0.2-0.4%,

[0067] Fungicide 0.1-0.2%,

[0068] Elastic emulsion 38-48%,

[0069] 500~700 mesh barium sulfate 5-8%,

[0070] 300~500 mesh talcum powder 8-10%;

[0071] 300-350 mesh heavy calcium powder 30-40%,

[0072] The second defoamer 0.1-0.3%,

[0073] Thickener 0.2-0.4%,

[0074] The second part of water 0.2-0.4%;

[0075] Leveling agent 0.1-0.3%,

[0076] The third part of water is 0.5-1%;

[0077] (2) Put the first part of water into the stirring device, start the stirrin...

Embodiment 2

[0113] Embodiment 2: a kind of product that above-mentioned anti-cracking waterproof middle layer paint preparation method makes, its each component and weight percentage thereof are as follows:

[0114] The first part of water is 8%,

[0115] Cellulose 0.4%,

[0116] Ethylene glycol 2%,

[0117] AMP-950.1%,

[0118] Dispersant 0.2%,

[0119] The first defoamer 0.2%,

[0120] Preservatives 0.2%,

[0121] Fungicide 0.1%,

[0122] Elastic emulsion 38%,

[0123] 500~700 mesh barium sulfate 5%,

[0124] 300~500 mesh talcum powder 10%,

[0125] 300~350 mesh heavy calcium powder 34%,

[0126] The second defoamer 0.1%,

[0127] Thickener 0.3%,

[0128] The second part of water is 0.3%,

[0129] Leveling agent 0.1%,

[0130] The third part of water 1%;

Embodiment 3

[0131] Embodiment 3: It differs from Embodiment 2 in that the components in the product and their weight percentages are different. Its each component and weight percentage thereof are as follows:

[0132] The first part of water is 5%,

[0133] Cellulose 0.2%,

[0134] Ethylene glycol 1.5%,

[0135] AMP-950.2%,

[0136] Dispersant 0.3%,

[0137] The first defoamer 0.4%,

[0138] Preservatives 0.3%,

[0139] Fungicide 0.2%,

[0140] Elastic emulsion 47%,

[0141] 500~700 mesh barium sulfate 5.5%,

[0142] 300~500 mesh talcum powder 8%,

[0143] 300~350 mesh heavy calcium powder 30%,

[0144] The second defoamer 0.2%,

[0145] Thickener 0.2%,

[0146] The second part of water is 0.2%,

[0147] Leveling agent 0.3%,

[0148] The third part of water is 0.5%,

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses an anti-cracking water-resistant intermediate paint preparation method and a product prepared by the method. The elastic emulsion used in the product is Tianba 2000, which has excellent water resistance, flexibility, alkali resistance and percentage of elongation. Assistants are common assistants for construction paints; and fillers are barium sulfate, talcum powder and coarse whiting powder, and the coarse fillers can enhance the physical and chemical properties of the coated film and lower the cost. The method disclosed by the invention has the advantages of simple preparation technique and high production efficiency, and is easy to implement. The anti-cracking water-resistant intermediate paint product disclosed by the invention has the advantages of favorable flexibility, strong cracking resistance (can bridge a 0.5-3mm crack), favorable water resistance, high binding firmness, favorable comprehensive properties, high temperature tolerance and high weather resistance, effectively solves the phenomena of cracking and water leakage in the walling, and ensures the walling to have neat and elegant appearance; and besides, the construction process is simple, greatly shortens the construction period, enhances the construction efficiency, requires low cost, and is beneficial to wide popularization.

Description

technical field [0001] The invention belongs to the technical field of paints, and in particular relates to a preparation method of an anti-cracking waterproof middle paint and products obtained by implementing the method. Background technique [0002] At present, in construction and painting engineering, intermediate paints are generally used. Although they can meet the general requirements for use, they do not have anti-cracking and waterproof functions. For example, the wall of a building has just been painted, and not long after, the wall cracks and the wall leaks, which seriously affects the paint coating effect. [0003] Along with the vigorous development of the construction and painting industry, the preparation method of the original intermediate paint is slow, the construction period is long, the anti-cracking and waterproof functions are poor, and the cost is high. Therefore researching and developing a kind of anti-cracking waterproof middle paint is the needs o...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09D201/00C09D7/12C09D5/00
Inventor 张立功
Owner 黄明杰
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products