A technology for lithographic ink and kaolin, which is applied in the field of preparation of high-concentration kaolin lithographic ink produced by a secondary kneading method, can solve the problems affecting ink production efficiency and cost, ink gloss, decreased fluidity, difficulty in using kaolin in large quantities, and the like. Excellent gloss and flow properties, shortened production time, and reduced grinding times

Active Publication Date: 2013-04-03
茂名阪田油墨有限公司
View PDF2 Cites 3 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] However, kaolin is difficult to finely disperse. During the mixing process of kaolin and pigment binder, due to the influence of temperature and other conditions, the dispersibility of the diluted ink produced is poor. When entering the next grinding process, it is necessary to increase the number of times of grinding. The fineness of the diluted ink is controlled within the acceptable range, resulting in low ink production efficiency and high cost; on the other hand, in the existing technology, the kaolin diluted ink and the colored pigment base ink are produced separately, and the process is complicated, so that It affects the production efficiency and cost of the ink; moreover, because kaolin itself contains water-soluble components, when the amount of kaolin added increases, that is to say, with the increase of the amount of kaolin ink added, ink glossiness, fluidity, etc. will occur. The decline in quality will lead to problems such as paste and ink accumulation in actual printing. Therefore, it is very difficult to use a large amount of kaolin in lithographic inks, which limits the amount of kaolin added, and it is difficult to reduce the cost of ink.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0072] A preparation method for producing high-concentration kaolin lithographic ink by secondary kneading method comprises the following preparation steps:

[0073] Step 1, kneading dry kaolin powder and coloring pigment once:

[0074] According to the percentage by weight, 8% of dry kaolin powder, 20% of C.I. Pigment Red 57:1 filter cake pigment and 37% of pigment binder were respectively added to the kneader for mixing and stirring. The stirring time was 25min and the kneading temperature was 65°C. Then carry out displacement dehydration, after standing for a period of time to separate the oil and water, tilt the kneader and pour out the water in the upper layer to obtain a kneaded mixture;

[0075] Specifically, the colored pigment is filter cake pigment or carbon black pigment, wherein the filter cake pigment is any one of C.I. Pigment Red 57:1 filter cake pigment, C.I. Pigment Yellow 12 filter cake pigment, and C.I. Pigment Blue 15:3 filter cake pigment kind;

[0076] ...

Embodiment 2

[0095] Its main technical scheme of the present embodiment is identical with embodiment 1, and difference is: the preparation method of producing high-concentration kaolin lithographic ink by secondary kneading method comprises the following preparation steps:

[0096] Step 1, kneading dry kaolin powder and coloring pigment once:

[0097] According to the percentage by weight, 14% of dry kaolin powder, 17.5% of C.I. Pigment Yellow 12 filter cake pigment and 28% of pigment binder were added to the kneader for mixing and stirring. The stirring time was 30min and the kneading temperature was 60°C, and then Replacement dehydration: After standing for a period of time to separate the oil and water, tilt the kneader to pour out the water in the upper layer to obtain a kneaded mixture;

[0098] Step 2, secondary kneading:

[0099] Add 80% of the soft water of the total weight of the primary kneaded mixture described in step 1 into the kneader, and then mix and stir again. After stir...

Embodiment 3

[0110] Its main technical scheme of the present embodiment is identical with embodiment 1, and difference is: the preparation method of producing high-concentration kaolin lithographic ink by secondary kneading method comprises the following preparation steps:

[0111] Step 1, kneading dry kaolin powder and coloring pigment once:

[0112] In percentage by weight, 18% of dry kaolin powder, 15% of C.I. Pigment Black 7 and soft water are mixed in a ratio of 1:1, and 30% of the pigment binder is added to the kneader for mixing and stirring. Kneading temperature is 20min, kneading temperature is 70°C, and then displacement dehydration: After standing for a period of time to separate oil and water, tilt the kneader to pour out the upper layer of water to obtain a kneaded mixture;

[0113] Step 2, secondary kneading:

[0114] Add 100% of the soft water of the total weight of the primary kneaded mixture described in step 1 into the kneader, and then mix and stir again. After stirring...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to the technical field of planographic printing ink, in particular to a preparation method of producing high-concentration kaolin planographic printing ink by adopting a secondary kneading method. The preparation method comprises the following specific steps: mixing mixed base ink, pigment connecting materials, friction-proof auxiliaries and ink oil, wherein the mixed base ink adopts secondary kneading technique, high-concentration kaolin and moisture-containing tinting pigment are added for first-time kneading, and soft water is added for secondary kneading after the replacement and dewatering are conducted. Compared with the prior art, according to the preparation method, the production technique is simplified, the production efficiency can be improved, the problems of declining qualities such as the brightness, flowability of the ink, and the like can also be stopped even if the content of the kaolin in the ink is increased, so that the addition amount of the kaolin with lower cost can be increased, the planographic printing ink with good dispersity and excellent brightness and flowability properties can be prepared, the production cost can be further lowered, thereby having better market prospects.

Description

technical field [0001] The invention relates to the technical field of lithographic inks, in particular to a preparation method for producing high-concentration kaolin lithographic inks by a secondary kneading method. Background technique [0002] In the prior art, in order to adjust the fluidity and viscosity of the ink and improve the printing adaptability of the ink when producing lithographic inks, it is usually necessary to use inorganic pigments such as calcium carbonate, clay, silica or kaolin. Diluted ink and colored pigment-based ink are prepared in two steps, that is, the inorganic pigment and pigment binder are mixed and ground to prepare diluted ink, and then the colored pigment and pigment binder are stirred, ground, dehydrated, etc. The first process is to prepare the colored pigment-based ink, and finally the diluted ink is further mixed with the colored pigment-based ink, and the ink with the desired properties is prepared through a series of adjustment proce...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C09D11/10C09D11/06C09D11/037
Inventor 荒木隆史建入实吴国蓬
Owner 茂名阪田油墨有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products