Water-based carpet glue and production method
A production method, carpet adhesive technology, applied in adhesive types, ester copolymer adhesives, etc., can solve problems such as unsafe transportation, toxic gas, explosion, etc., to ensure transportation safety, save funds, and reduce product costs Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Pre-emulsification: mix 110kg of deionized water, 4.0kg of emulsifier sodium dodecylsulfonate, 6.4kg of emulsifier CA-897, 7kg of crosslinking agent N, N--dimethylolacrylamide, and mix well in Slowly add the pre-weighed and mixed functional monomer 5.5kg methacrylic acid, 18kg acrylonitrile, 93.5kg styrene, 84kg methyl acrylate, 216kg butyl acrylate, and stir well while stirring at 600 rpm The pre-emulsified monomer was obtained, and 136 kg was separated for use;
[0023] Cleaning: After rinsing the reactor, inject 410kg of deionized water, 1.0kg of emulsifier sodium dodecylsulfonate and 1.6kg of emulsifier CA-897 according to the formula ratio, turn on the stirring, and turn on the heating or cooling water device;
[0024] Heating: raise the temperature to 60°C, put 136kg of the separated emulsified monomer into the kettle, continue to heat up to 80°C, put in one-third of the initiator solution (1.3kg of ammonium persulfate + 30kg of deionized water), and raise the tem...
Embodiment 2
[0029] Pre-emulsification: Mix 100kg of deionized water, 4.4kg of emulsifier sodium dodecyl sulfonate, 7.2kg of emulsifier CA-897, 8kg of cross-linking agent N, N--dimethylolacrylamide, in Slowly add 4kg methacrylic acid, 21kg acrylonitrile, 100kg styrene, 70kg butyl acrylate, 280kg ethyl acrylate, the pre-weighed and mixed functional monomer into the stirring at 550 rpm, and stir well The pre-emulsified monomer was obtained, and 148 kg was separated for use;
[0030] Cleaning: After rinsing the reactor, inject 370kg of deionized water, 1.1kg of emulsifier sodium dodecylsulfonate and 1.8kg of emulsifier CA-897 according to the formula ratio, turn on the stirring, and turn on the heating or cooling water device;
[0031] Heating: raise the temperature to 55°C, put 148kg of the separated emulsified monomer into the kettle, continue to heat up to 75°C, put in one-third of the initiator solution (2kg of ammonium persulfate + 30kg of deionized water), and raise the temperature unt...
Embodiment 3
[0036] Pre-emulsification: Mix 120kg of deionized water, 4.8kg of emulsifier sodium dodecylsulfonate, 8kg of emulsifier CA-897, 6kg of cross-linking agent N, N--dimethylolacrylamide, and mix well in Slowly add the pre-weighed and mixed functional monomers 6kg methacrylic acid, 89kg styrene, 10kg acrylonitrile, 30kg methyl acrylate, 250kg ethyl acrylate, and stir well The pre-emulsified monomer was obtained, and 130 kg was separated for use;
[0037] Cleaning: After rinsing the reactor, inject 450kg of deionized water, 1.2kg of emulsifier sodium dodecylsulfonate and 2kg of emulsifier CA-897 according to the formula ratio, turn on the stirring, and turn on the heating or cooling water device;
[0038] Heating: raise the temperature to 65°C, put 130kg of the separated emulsified monomer into the kettle, continue to heat up to 85°C, put in one-third of the initiator solution (1kg of potassium persulfate + 30kg of deionized water), and raise the temperature until the emulsion beco...