[0013] A method for preparing an anti-dripping agent, comprising the steps of:
[0014] 1) Mix 1.2 parts by mass of acrylonitrile, 10 parts by mass of styrene, 1 part by mass of imidazoline, 2 parts by mass of dodecyltrimethylammonium chloride, 6 parts by mass of methacrylic acid, 1 part by mass of dodecyl trimethylammonium Methyl ammonium bromide, 3 parts by mass of butadiene, 7 parts by mass of butyl methacrylate, 2 parts by mass of tetramethylammonium bromide, 1 part by mass of ammonium persulfate, 5 parts by mass of methyl methacrylate, 2 parts by mass Part of azobisisoheptanonitrile, 1 mass part of benzoyl peroxide, 1 mass part of potassium persulfate, 1 mass part of dodecyl trimethylammonium sulfate, 1 mass part of azobisisobutyronitrile mixed and stirred to obtain pre-emulsion;
[0015] 2) Add 65 parts by mass of deionized water to the pre-emulsion, mix well, keep the speed at 150r / min, raise the temperature to 90°C at 5°C / min, polymerize for 12 hours, cool to room tem...
Embodiment 2
[0019] A method for preparing an anti-dripping agent, comprising the steps of:
[0020] 1) Mix 2 parts by mass of acrylonitrile, 10 parts by mass of styrene, 1 part by mass of imidazoline, 2 parts by mass of dodecyltrimethylammonium chloride, 6 parts by mass of methacrylic acid, 1 part by mass of dodecyltrimethylammonium Methyl ammonium bromide, 3 parts by mass of butadiene, 7 parts by mass of butyl methacrylate, 2 parts by mass of tetramethylammonium bromide, 1 part by mass of ammonium persulfate, 5 parts by mass of methyl methacrylate, 2 parts by mass Part of azobisisoheptanonitrile, 1 mass part of benzoyl peroxide, 1 mass part of potassium persulfate, 1 mass part of dodecyl trimethylammonium sulfate, 1 mass part of azobisisobutyronitrile mixed and stirred to obtain pre-emulsion;
[0021] 2) Add 65 parts by mass of deionized water to the pre-emulsion, mix well, keep the speed at 150r / min, raise the temperature to 90°C at 5°C / min, polymerize for 12 hours, cool to room temper...
Embodiment 3
[0025] A method for preparing an anti-dripping agent, comprising the steps of:
[0026] 1) Mix 1 part by mass of acrylonitrile, 10 parts by mass of styrene, 1 part by mass of imidazoline, 2 parts by mass of dodecyltrimethylammonium chloride, 6 parts by mass of methacrylic acid, 1 part by mass of dodecyltrimethylammonium Methyl ammonium bromide, 3 parts by mass of butadiene, 7 parts by mass of butyl methacrylate, 2 parts by mass of tetramethylammonium bromide, 1 part by mass of ammonium persulfate, 5 parts by mass of methyl methacrylate, 2 parts by mass Part of azobisisoheptanonitrile, 1 mass part of benzoyl peroxide, 1 mass part of potassium persulfate, 1 mass part of dodecyl trimethylammonium sulfate, 1 mass part of azobisisobutyronitrile mixed and stirred to obtain pre-emulsion;
[0027] 2) Add 65 parts by mass of deionized water to the pre-emulsion, mix well, keep the speed at 150r / min, raise the temperature to 90°C at 5°C / min, polymerize for 12 hours, cool to room tempera...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More