Method for reducing dust content of down feather
A down and dust technology, which is applied in textiles and papermaking, fiber treatment, dry cleaning fiber products, etc., can solve the problems of down structure damage, poor dust removal effect, etc., and achieve the effects of reducing damage, enhancing mobility, and reducing friction coefficient
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] 1) Add down, water, and detergent into the washing machine to wash the down. Among them, the mass ratio of water to down is 20:1, the washing temperature is 40°C, the mass of detergent added per liter of water is 1g, and it is rotated for 20 minutes.
[0032] 2) Rinse the washed down to remove detergent.
[0033] 3) Adjust the mass ratio of water to rinsed down in the washing machine to 20:1, and after the temperature is 60°C, add softener sulfated castor oil, and adjust the pH value to 4.0 with 0.1g / L formic acid after rotating for 50 minutes. Rotate 30 minutes; Wherein, the quality that adds softening agent sulfated castor oil in every liter of water is 1g;
[0034] 4) Drying, drying, and packaging the down treated in step 3) to obtain down and down with reduced dust.
Embodiment 2
[0036] 1) Add down, water, and detergent into the washing machine to wash the down. Among them, the mass ratio of water to down is 20:1, the washing temperature is 50°C, the mass of detergent added per liter of water is 2g, and it is rotated for 25 minutes.
[0037] 2) Rinse the washed down to remove detergent.
[0038] 3) Adjust the mass ratio of water and rinsed down in the washing machine to 30:1. After the temperature is 60°C, add the softener lanolin succinate sulfonate, and adjust the pH value with 2g / L hydrochloric acid after rotating for 10 minutes. 3.5, rotate for 20 minutes; wherein, the quality of the softening agent lanolin succinate sulfonate added per liter of water is 3g.
[0039] 4) Drying, drying, and packaging the down treated in step 4) to obtain down and down with reduced dust.
Embodiment 3
[0041] 1) Add down, water, and detergent into the washing machine to wash the down. Among them, the mass ratio of water to down is 35:1, the washing temperature is 40°C, the mass of detergent added to each liter of water is 2.5g, and it is rotated for 25 minutes.
[0042] 2) Rinse the washed down to remove detergent.
[0043] 3) Adjust the mass ratio of water in the washing machine to the rinsed down to 20:1, and after the temperature is 50°C, add the softener pentadecylsulfonyl chloride, rotate for 20 minutes, and adjust the pH value to 3.5 with 1g / L sulfuric acid. Rotate for 20 minutes; Wherein, the quality that the softening agent pentadecylsulfonyl chloride is added in every liter of water is 2g.
[0044] 4) Drying, drying, and packaging the down treated in step 3) to obtain down and down with reduced dust.
PUM