A water-based and coating technology, applied in the direction of coating, etc., can solve the problems of single sensory effect, poor stability of color particles, long production cycle, etc., and achieve the effect of high stability of color particles, controllable size of color particles, and short production cycle
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] The water-based rock color paint comprises the following raw materials in parts by weight: 40 parts of base paint, 20 parts of protective glue, and 20 parts of synthetic emulsion. The following raw materials are commercially available.
[0033] The base paint contains the following raw materials in parts by weight: 20 parts of water-based fluorocarbon emulsion, 20 parts of ionized water, 3 parts of non-ionic polyurethane dispersant, 1 part of wetting agent (X-405), 10 parts of gel, pigment (R -902) 10 parts, filler (600 mesh heavy calcium) 5 parts, fungicide 0.1 part, defoamer (NX202) 0.2 part, thickener (TT-615) 0.3 part.
[0034] Protective glue: 20 parts of polyvinyl alcohol.
[0035] The synthetic emulsion contains the following raw materials in parts by weight: 10 parts of anionic synthetic resin solution, 2 parts of calcium salt, 1 part of propylene glycol and 80 parts of water.
[0036] The preparation of this kind of water-based rock color paint:
[0037] (1)...
Embodiment 2
[0042] The water-based rock color paint comprises the following raw materials in parts by weight: 50 parts of base paint, 30 parts of protective glue and 30 parts of synthetic emulsion. The following raw materials are commercially available.
[0043] The base paint contains the following raw materials in parts by weight: 30 parts of water-based fluorocarbon emulsion, 30 parts of ionized water, 5 parts of non-ionic polyurethane dispersant, 3 parts of wetting agent (X-405), 15 parts of gel, pigment (R -902) 15 parts, filler (600 mesh heavy calcium) 10 parts, fungicide 0.2 parts, defoamer (NX202) 0.3 parts, thickener (TT-615) 0.6 parts.
[0044] Protective glue: 30 parts of polyvinyl alcohol.
[0045] The synthetic emulsion includes the following raw materials in parts by weight: 20 parts of anionic synthetic resin solution, 4 parts of calcium salt, 2 parts of propylene glycol, and 90 parts of water.
[0046] The preparation of this kind of water-based rock color paint:
...
Embodiment 3
[0052] The water-based rock color paint comprises the following raw materials in parts by weight: 45 parts of base paint, 25 parts of protective glue, and 25 parts of synthetic emulsion. The following raw materials are commercially available.
[0053] The base paint contains the following raw materials in parts by weight: 25 parts of water-based fluorocarbon emulsion, 25 parts of ionized water, 4 parts of non-ionic polyurethane dispersant, 2 parts of wetting agent (X-405), 12 parts of gel, pigment (R -902) 12 parts, filler (600 mesh heavy calcium) 7 parts, fungicide 0.1 part, defoamer (NX202) 0.2 part, thickener (TT-615) 0.4 part.
[0054] Protective glue: 25 parts of polyvinyl alcohol.
[0055] The synthetic emulsion contains the following raw materials in parts by weight: 15 parts of anionic synthetic resin solution, 3 parts of calcium salt, 1 part of propylene glycol, and 85 parts of water.
[0056] The preparation of this kind of water-based rock color paint:
[0057] (...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com