A fiber blended and knitted fabric technology, used in fiber processing, dry cleaning fiber products, textiles and papermaking, etc., can solve the problems of energy consumption and complicated process steps, reduce process time and energy consumption, and achieve stable product quality. Reasonable effect of dyeing process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
specific Embodiment 1
[0014] A dyeing and finishing process of wrinkle-resistant fiber blended knitted fabrics comprises the following steps: sizing-desizing-scouring-dyeing-soaping.
[0015] The sizing: pre-wet treatment is carried out before sizing the blended yarn. The parameters of the pre-wet treatment are: the temperature of the pre-wet tank is 40°C; the pre-wet press force is 50KN; rate of 7%, nip roll pressure 0.3mPa, bath roll pressure 0.45mPa, water content 0.7%, the slurry formula is: grafted starch 94wt%, smoothing agent 1.2wt%, penetrating agent 0.6wt%, anti- Static agent 0.8wt%.
[0016] The desizing: fabric padding desizing solution, adding 9g / L oxidation desizing solution, 4g / L chelating dispersant, and 350g / L liquid caustic soda to the desizing solution.
[0017] Said dyeing: configure the dye liquor with a bath ratio of 1:6, first add 38°C water, then add a chelating dispersant, a leveling agent and a pH value buffer in the water, and heat up the dye liquor at a heating rate of 1...
specific Embodiment 2
[0021] A dyeing and finishing process of wrinkle-resistant fiber blended knitted fabrics comprises the following steps: sizing-desizing-scouring-dyeing-soaping.
[0022] The sizing: pre-wet treatment is carried out before sizing the blended yarn. The pre-wet treatment parameters are: pre-wet tank temperature 80°C; pre-wet press force 78KN; sizing temperature 55°C, sizing speed 38m / min, sizing Rate 9%, nip roll pressure 0.3mPa, bath roll pressure 0.45mPa, moisture content 0.7%, described slurry formula is: grafted starch 96wt%, smoothing agent 1.8wt%, penetrating agent 1.3wt%, anti- Static agent 0.8wt%.
[0023] The desizing: fabric padding desizing solution, adding 13g / L oxidation desizing solution, 8g / L chelating dispersant, and 410g / L liquid caustic soda to the desizing solution.
[0024] Said dyeing: configure the dye liquor with a liquor ratio of 1:6, first add 46°C water, then add a chelating dispersant, a leveling agent and a pH value buffer in the water, and heat up th...
specific Embodiment 3
[0028] A dyeing and finishing process of wrinkle-resistant fiber blended knitted fabrics comprises the following steps: sizing-desizing-scouring-dyeing-soaping.
[0029] The sizing: pre-wet treatment is carried out before sizing the blended yarn. The pre-wet treatment parameters are: pre-wet tank temperature 60°C; pre-wet press force 64KN; sizing temperature 39°C, sizing speed 34m / min, sizing Rate 8%, nip roll pressure 0.3mPa, bath roll pressure 0.45mPa, water content 0.7%, described slurry formula is: grafted starch 95wt%, smoothing agent 1.5wt%, penetrant 0.9wt%, anti- Static agent 0.8wt%.
[0030] Described desizing: fabric padding desizing liquid, desizing liquid adds 11g / L oxidation desizing liquid, 6g / L chelating dispersant, 380g / L liquid caustic soda.
[0031] Said dyeing: configure the dye liquor with a bath ratio of 1:6, first add 43°C water, then add a chelating dispersant, a leveling agent and a pH value buffer in the water, and heat up the dye liquor at a heating ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com