High-precision air filter paper as well as preparation method and application thereof
An air filter paper, high-precision technology, applied in the field of filter paper, can solve the problems of poor air filter paper bulk, uneven fiber thickness, low filtration accuracy, etc., to achieve the effect of increasing water resistance, simple production process, and reducing production costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] A manufacturing process of high-precision air filter paper, comprising the steps of:
[0043] 1) Add 8% NaOH to 15 kg of linter pulp, stir at 120°C for 4 hours to fully remove the wax and soluble impurities in the linters; the viscosity of the linter pulp after treatment is 300 mPas, and the α-fiber The element content is 98%, the ash content is 0.2%;
[0044] 2) Treat the linter pulp obtained in 1) with 5% HCl at room temperature for 3 hr;
[0045] 3) The cotton linter pulp and polylactic acid fibers in step 2) are beaten with a beater, and then online polished by a double-disk refiner to obtain a slurry with a beating concentration of 1.98%, and beating to 16°SR and 22°SR respectively;
[0046] 4) glass fibers are added to the slurry obtained in step 3) to form a pulp slurry;
[0047] 5) Dilute 2 kg of polyamide polyepichlorohydrin resin with water, stir evenly, and slowly add it to the pulp slurry;
[0048] 6) 3 kg of butanol, 3 kg of carboxymethyl cellulose, 1 kg...
Embodiment 2
[0054] A manufacturing process of high-precision air filter paper, comprising the steps of:
[0055] 1) Add 12% NaOH to 18kg of linter pulp, stir at 140°C for 4 hours to fully remove the wax and soluble impurities in the linters; the viscosity of the linter pulp after treatment is 290mPas, and the α-fiber The element content is 99%, the ash content is 0.3%;
[0056]2) Treat the linter pulp obtained in 1) with 8% HCl at room temperature for 3 hr;
[0057] 3) The cotton linter pulp and polylactic acid fibers in step 2) are beaten with a beater, and then online polished by a double-disc refiner to obtain a slurry with a beating concentration of 2.67%, and beating to 15°SR and 26°SR respectively;
[0058] 4) glass fibers are added to the slurry obtained in step 3) to form a pulp slurry;
[0059] 5) Dilute 2 kg of polyamide polyepichlorohydrin resin with water, stir evenly, and slowly add it to the pulp slurry;
[0060] 6) 4kg of silicone oil, 4kg of sodium hexametaphosphate, 2k...
Embodiment 3
[0066] A manufacturing process of high-precision air filter paper, comprising the steps of:
[0067] 1) Add 10% NaOH to 12kg of linter pulp, stir at 120°C for 4 hours to fully remove wax and soluble impurities in linters; the viscosity of the linter pulp after treatment is 280mPas, and α-fiber The element content is 98.5%, the ash content is 0.2%;
[0068] 2) Treat the linter pulp obtained in 1) with 6% HCl at room temperature for 3 hr;
[0069] 3) The cotton linter pulp and polylactic acid fibers in step 2) are beaten with a beater, and then online polished by a double-disc refiner to obtain a slurry with a beating concentration of 2.08%, and beating to 18°SR and 20°SR respectively;
[0070] 4) glass fibers are added to the slurry obtained in step 3) to form a pulp slurry;
[0071] 5) Dilute 2 kg of polyamide polyepichlorohydrin resin with water, stir evenly, and slowly add it to the pulp slurry;
[0072] 6) 3 kg of pine oil, 3 kg of sodium pyrophosphate, 0.5 kg of waterpr...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com