Preparing method for electrostatic type air purifier dust collecting plates
An air purifier and dust collecting board technology, which is applied in the field of dust collecting board preparation, can solve the problems of electric breakdown of metal plates, reduced dust collection efficiency, ozone generation, etc., and achieves mild synthesis conditions, long service life, and dust collection. good effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] (1) Pretreatment
[0035] a. Take a 15cm×4cm polypropylene plate and ultrasonically clean it in acetone solution for 15 minutes;
[0036] b. Dilute 9.48g of potassium permanganate solid powder to 100mL with water and stir evenly; take 1.1mL of 98% sulfuric acid and dilute to 100mL with water, mix the two solutions to obtain an oxidation treatment solution.
[0037] c. Immerse the polypropylene plate in the oxidation treatment solution, and seal the mouth of the beaker with a plastic film;
[0038] d. Place the beaker in a constant temperature magnetic stirring water bath and treat it at 60°C for 6 hours;
[0039] e. Take out the polypropylene plate, remove the floating color with oxalic acid, wash it thoroughly with deionized water, and dry it.
[0040] (2) In-situ polymerized polyaniline
[0041] f. Cover the front and rear surfaces of the polypropylene board with tape, and leave a 1cm width in the middle of the front to polymerize polyaniline;
[0042] g. Dilute 1...
Embodiment 2
[0052] (1) Pretreatment
[0053] a. Take a 15cm×4cm polypropylene plate and ultrasonically clean it in acetone solution for 15 minutes;
[0054] b. Dilute 9.48g of potassium permanganate solid powder to 100mL with water and stir evenly; take 1.1mL of 98% sulfuric acid and dilute to 100mL with water, mix the two solutions to obtain an oxidation treatment solution.
[0055] c. Immerse the polypropylene plate in the oxidation treatment solution, and seal the mouth of the beaker with a plastic film;
[0056] d. Place the beaker in a constant temperature magnetic stirring water bath and treat it at 60°C for 6 hours;
[0057] e. Take out the polypropylene plate, remove the floating color with oxalic acid, wash it thoroughly with deionized water, and dry it.
[0058] (2) In-situ polymerized polyaniline
[0059] f. Dilute 17.4ml of hydrochloric acid to 75mL with water, then dilute 10ml of aniline to 75mL with water, mix the two solutions, stir well, and make aniline / hydrochloric acid...
Embodiment 3
[0069] (1) Pretreatment
[0070] a. Take a 10cm×10cm polypropylene film, and ultrasonically clean it in acetone solution for 15 minutes;
[0071] b. Dilute 9.48g of potassium permanganate solid powder to 100mL with water and stir evenly; take 1.1mL of 98% sulfuric acid and dilute to 100mL with water, mix the two solutions to obtain an oxidation treatment solution.
[0072] c. Immerse the polypropylene film in the oxidation treatment solution, and seal the mouth of the beaker with a plastic film;
[0073] d. Place the beaker in a constant temperature magnetic stirring water bath and treat it at 60°C for 6 hours;
[0074] e. Take out the polypropylene film, remove the floating color with oxalic acid, wash it thoroughly with deionized water, and dry it.
[0075] (2) In-situ polymerized polyaniline
[0076] f. Dilute 17.4ml of hydrochloric acid to 75mL with water, then dilute 10ml of aniline to 75mL with water, mix the two solutions, stir well, and make aniline / hydrochloric aci...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com