A temperature change, black technology, applied in the field of black temperature change paint, can solve the problems of high equipment temperature, shortened equipment life, paint peeling on equipment surface, etc., and achieves the effect of low heavy metal content, good environmental protection and bright colors
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0090] Resin percentage:
[0091] (1) Polyurethane resin 24%
[0092] (2) Thermoplastic acrylic resin 10%
[0093] (3) Fully etherified amino resin 5%
[0094] Pigment percentage:
[0095] (1) Electron transfer organic compound 25%
[0096] Solvent Percentage:
[0097] (1) Cyclohexanone 5%
[0098] (2) Xylene 8%
[0099] (3) Butyl ester 12%
[0100] (4) MIBK 9%
[0101] Auxiliary percentage:
[0102] (1) Fluorine modified leveling agent 1%
[0103] (2) Silicon defoamer 2%
[0104] (3) Polymer copolymer alkyl ammonium salt dispersant 1%
[0105] The process steps are as follows:
[0106] A. First add the main resin and dispersant with reactive groups, part of the mixed solvent, and stir evenly at low speed (400-600r / min);
[0107] B. Add temperature-changing powder under stirring condition, disperse and wet at low speed (400-600r / min), this is the pre-pulp in the previous stage;
[0108] C. Grind the pre-pulp with a three-roll machine or a sand mill to a fineness ...
Embodiment 2
[0121] Resin percentage:
[0122] (1) Polyurethane resin 24.5%
[0123] (2) Thermoplastic acrylic resin 9.5%
[0124] (3) Fully etherified amino resin 5%
[0125] Pigment percentage:
[0126] (1) Electron transfer organic compounds 26%
[0127] Solvent Percentage:
[0128] (1) Cyclohexanone 4.5%
[0129] (2) Xylene 8.5%
[0130] (3) Butyl ester 11.5%
[0131] (4) MIBK 9.5%
[0132] Auxiliary percentage:
[0133] (1) Fluorine modified leveling agent 1.1%
[0134] (2) Silicon defoamer 2.3%
[0135] (3) Polymer copolymer alkyl ammonium salt dispersant 0.7%
[0136] The process steps are as follows:
[0137] A. First add the main resin and dispersant with reactive groups, part of the mixed solvent, and stir evenly at low speed (400-600r / min);
[0138] B. Add temperature-changing powder under stirring condition, disperse and wet at low speed (400-600r / min), this is the pre-pulp in the previous stage;
[0139] C. Grind the pre-pulp with a three-roll machine or a sand m...
PUM
Property | Measurement | Unit |
---|---|---|
Film thickness | aaaaa | aaaaa |
Hardness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com