A technology of neutral sizing agent and anionic monomer, applied in the direction of water-repellent addition, etc., can solve problems such as small slip coefficient, affect paper whiteness, strong dependence on aluminum sulfate, etc., achieve strong emulsification ability and improve paper formation quality effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0035] The preparation method of anionic liquid AKD neutral sizing agent, according to the following steps:
[0036] 1) Add 15g polyvinyl alcohol and 350g distilled water into a three-necked flask equipped with stirring;
[0037] 2) Add 10g of styrene, 5g of butyl acrylate, 5g of tert-butyl acrylate, 50g of acrylamide, and 20g of acrylic acid into a three-necked flask;
[0038] 3) Adjust the pH to 3 with glacial acetic acid, stir and mix for 0.5h, then raise the temperature to 85°C;
[0039] 4) Add 30g ammonium persulfate solution (0.1% total monomer mass) dropwise within 1.5h;
[0040] 5) Heat up to 95°C and keep it warm for 3 hours, then cool and discharge to obtain a light yellow viscous substance, which is the anionic polymer emulsifier for liquid AKD;
[0041] 6) Add 50g of liquid AKD, 50g of special anionic polymer emulsifier for liquid AKD and 50g of distilled water into a three-necked flask with stirring;
[0042] 7) Heat up to 35°C;
[0043] 8) Adjust the speed to...
Embodiment 2
[0046] The preparation method of anionic liquid AKD neutral sizing agent, according to the following steps:
[0047] 1) Add 20g sodium polyacrylate and 350g distilled water into a three-neck flask equipped with stirring;
[0048] 2) Add 10g of styrene, 7.5g of butyl methacrylate, 7.5g of isobutyl methacrylate, 60g of acrylamide, 15g of acrylic acid and 5g of itaconic acid into a three-necked flask;
[0049] 3) Adjust the pH to 5 with glacial acetic acid, and raise the temperature to 90°C;
[0050] 4) Add 30g ammonium persulfate solution (0.1% total monomer mass) dropwise within 1.5h;
[0051] 5) Raise the temperature to 95°C and keep it warm for 2 hours, then cool and discharge to obtain a light yellow viscous substance, which is the anionic polymer emulsifier for liquid AKD;
[0052] 6) Add 50g of liquid AKD, 50g of special anionic polymer emulsifier for liquid AKD and 50g of distilled water into a three-necked flask with stirring;
[0053] 7) Control the temperature to 30°C...
Embodiment 3
[0057] The preparation method of anionic liquid AKD neutral sizing agent, according to the following steps:
[0058] 1) Add 20g polyethylene glycol and 350g distilled water into a three-necked flask equipped with stirring;
[0059] 2) Add 20g of styrene, 5g of ethyl acrylate, 5g of isooctyl methacrylate, 50g of acrylamide, and 20g of styrenesulfonic acid into a three-necked flask;
[0060] 3) Adjust the pH to 4 with glacial acetic acid and raise the temperature to 85°C;
[0061] 4) Add 30g ammonium persulfate solution (0.1% total monomer mass) dropwise within 1.5h;
[0062] 5) Raise the temperature to 95°C and keep it warm for 2 hours, then cool and discharge to obtain a light yellow viscous substance, which is the anionic polymer emulsifier for liquid AKD;
[0063] 6) Add 50g of liquid AKD, 50g of special anionic polymer emulsifier for liquid AKD and 50g of distilled water into a three-necked flask with stirring;
[0064] 7) Heat up to 35°C;
[0065] 8) Adjust the speed t...