Drilling fluid filtrate reducer and preparation method thereof
A technology of fluid loss reducer and drilling fluid, which is applied in the field of petroleum drilling fluid, can solve the problems of insufficient compactness of filter cake, insufficient plugging capacity of rock micropores and micro-fractures, and increased risk of shale well wall collapse, etc., to achieve improved Tightness, improve wellbore stability, and improve the effect of fluid loss reduction
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] The fluid loss control agent used in this embodiment comprises the following components in 100 parts by weight:
[0022] 70 parts by weight of heavy liquid paraffin;
[0023] Span80 10 parts by weight;
[0024] 20 parts by weight of nano silicon dioxide and nano calcium carbonate aqueous dispersion.
[0025] The preparation method that present embodiment uses described nano silicon dioxide and nano calcium carbonate water dispersion liquid comprises:
[0026] Add nano-silica and nano-calcium carbonate to deionized water at a weight ratio of 2:1, then add sodium hexametaphosphate, and stir at a high speed for 30 minutes at 25°C to obtain an aqueous dispersion of nano-silica and nano-calcium carbonate.
[0027] The method for preparing the fluid loss control agent described in this embodiment includes:
[0028] Mix Span80 and heavy liquid paraffin at a weight ratio of 7:1, stir at 25°C with a magnetic stirrer at high speed for 10 min, then gradually add nano-silica and...
Embodiment 2
[0030] The fluid loss control agent used in this embodiment comprises the following components in 100 parts by weight:
[0031] 50 parts by weight of white oil;
[0032] Tween20 20 parts by weight;
[0033] 30 parts by weight of nano silicon dioxide and nano calcium carbonate aqueous dispersion.
[0034] The preparation method that present embodiment uses described nano silicon dioxide and nano calcium carbonate water dispersion liquid comprises:
[0035] Add nano-silica and nano-calcium carbonate into deionized water at a weight ratio of 3:2, then add sodium polyacrylate, and stir at 30°C for 60 minutes at high speed to obtain an aqueous dispersion of nano-silica and nano-calcium carbonate.
[0036] The method for preparing the fluid loss control agent described in this embodiment includes:
[0037] Mix Tween20 and white oil in a weight ratio of 5:2, stir at 30°C with a magnetic stirrer for 30 minutes at high speed, then gradually add nano-silica and nano-calcium carbonate...
Embodiment 3
[0039] The fluid loss control agent used in this embodiment comprises the following components in 100 parts by weight:
[0040] 60 parts by weight of heavy liquid paraffin;
[0041] 20 parts by weight of the mixture of Span80 and PVA;
[0042] 20 parts by weight of nano silicon dioxide and nano calcium carbonate aqueous dispersion.
[0043] The preparation method that present embodiment uses described nano silicon dioxide and nano calcium carbonate water dispersion liquid comprises:
[0044] Add nano-silica and nano-calcium carbonate into deionized water at a weight ratio of 1:1, then add a mixture of polyethylene glycol and sodium hexametaphosphate (mixing ratio 1:3), and stir at 40°C for 50 minutes at high speed to obtain Nano silicon dioxide and nano calcium carbonate aqueous dispersion.
[0045] The method for preparing the fluid loss control agent described in this embodiment includes:
[0046] Mix the mixture of Span80 and PVA (mixing ratio 4:1) with heavy liquid par...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com