A kind of fast-growing wood bending method
A fast-growing wood, bending technology, applied in the direction of wood bending, wood compression, wood impregnation, etc., can solve the problems of low physical and mechanical strength, low strength, hardness, uneven structure, etc., to improve the use value, stable properties, expansion Application-wide effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A fast-growing wood bending method, comprising the following steps:
[0023] S1: initial compression
[0024] Compressing the wood to be bent perpendicular to the grain;
[0025] S2: softening treatment
[0026] The initially compressed wood is placed in a softening solution for softening treatment, and the softening solution is made of the following components in parts by weight: 14 parts of sodium molybdate dihydrate, 4 parts of sodium 1-heptanesulfonate, chain extender 8 parts of HER, 2 parts of aluminum bromide, 300 parts of water;
[0027] S3: compression
[0028] Compress the softened wood along the grain;
[0029] S4: Curved
[0030] Evenly smear the bending aid on the convex surface after the bending of the wood, and then place the wood on a wood bending machine for bending to obtain a finished product. The bending aid is made of the following components by weight: 11 parts of behenamide, 14 parts of ethylene dioleamide, 5 parts of p-dodecylbenzenesulfonyl...
Embodiment 2
[0036] A fast-growing wood bending method, comprising the following steps:
[0037] S1: initial compression
[0038] Compressing the wood to be bent perpendicular to the grain;
[0039] S2: softening treatment
[0040] The initially compressed wood is placed in a softening solution for softening treatment, and the softening solution is made of the following components by weight: 16 parts of sodium molybdate dihydrate, 6 parts of sodium 1-heptanesulfonate, chain extender 9 parts of HER, 4 parts of aluminum bromide, 330 parts of water;
[0041] S3: compression
[0042] Compress the softened wood along the grain;
[0043] S4: Curved
[0044] Evenly smear a bending aid on the convex surface of the wood after bending, and then place the wood on a wood bending machine for bending to obtain a finished product. The bending aid is made of the following components by weight: 13 parts of behenamide, 16 parts of ethylene dioleamide, 7 parts of p-dodecylbenzenesulfonyl chloride, 15 p...
Embodiment 3
[0050] A fast-growing wood bending method, comprising the following steps:
[0051] S1: initial compression
[0052] Compressing the wood to be bent perpendicular to the grain;
[0053] S2: softening treatment
[0054] The initially compressed wood is placed in a softening solution for softening treatment, and the softening solution is made of the following components in parts by weight: 18 parts of sodium molybdate dihydrate, 7 parts of sodium 1-heptanesulfonate, chain extender 10 parts of HER, 6 parts of aluminum bromide, 350 parts of water;
[0055] S3: compression
[0056] Compress the softened wood along the grain;
[0057] S4: Curved
[0058] Evenly smear a bending aid on the convex surface of the wood after bending, and then place the wood on a wood bending machine for bending to obtain a finished product. The bending aid is made of the following components by weight: 16 parts of behenamide, 18 parts of ethylene dioleamide, 8 parts of p-dodecylbenzenesulfonyl chlo...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com