Embodiment 1
[0020] A preparation method of small particle size ABC dry powder fire extinguishing agent includes the following steps:
[0021] S1. Stir 60g nano calcium carbonate, 4g stearic acid, and 2g myristic acid for 20min at a stirring speed of 1600r / min. Add 16g microcrystalline paraffin and 80g water to mix evenly, add 10g sodium oleate sulfate under stirring, and heat to Stir at 90°C for 45 minutes, filter, wash, dry, and crush to obtain the first material;
[0022] S2. Mix 100g of monoammonium phosphate, 40g of potassium dihydrogen phosphate, 10g of potassium perchlorate, 12g of glass fiber, and 6g of the first material uniformly, and homogenize for 20 minutes at a homogenization pressure of 4kPa to obtain the second material;
[0023] S3. Mix 4g of hydrogen-containing silicone oil and 6g of water evenly, then add 8g of acetone and stir evenly to obtain a mixture; spray the mixture into 100g of the second material in a stirring state, heat up to 88℃ and mix evenly, remove the water , A...
Embodiment 2
[0025] A preparation method of small particle size ABC dry powder fire extinguishing agent includes the following steps:
[0026] S1. Stir 80g nano calcium carbonate, 2g stearic acid, 4g myristic acid for 10min at a stirring speed of 2000r / min, add 8g microcrystalline paraffin, 120g water and mix uniformly, add 4g sodium oleate sulfate under stirring, and heat to Stir at 96°C for 25 min, filter, wash, dry, and crush to obtain the first material;
[0027] S2. Mix 120kg of monoammonium phosphate, 20kg of potassium dihydrogen phosphate, 20kg of potassium perchlorate, 6kg of glass fiber, and 10kg of the first material uniformly, homogenize for 10 minutes, and homogenize pressure of 8kPa to obtain the second material;
[0028] S3. Mix 2kg of hydrogen-containing silicone oil and 12kg of water evenly, then add 4kg of acetone and stir evenly to obtain the mixture; spray the mixture into 160kg of the second material in a stirring state, heat up to 80℃ and mix evenly, remove the water , Add 2...
Embodiment 3
[0030] A preparation method of small particle size ABC dry powder fire extinguishing agent includes the following steps:
[0031] S1. Stir 65kg of nano calcium carbonate, 3.5kg of stearic acid, and 2.5kg of myristic acid for 18min at a stirring speed of 1700r / min. Add 14kg of microcrystalline paraffin and 90kg of water to mix evenly. Add 8kg of sulfated sodium oleate under stirring. Warm up to 92°C and stir for 40 minutes, filter, wash, dry, and crush to obtain the first material;
[0032] S2. Mix 105kg of monoammonium phosphate, 35kg of potassium dihydrogen phosphate, 12kg of potassium perchlorate, 10kg of glass fiber, and 7kg of the first material, homogenize for 18min, and homogenize pressure of 5kPa to obtain the second material;
[0033] S3. Mix 3.5kg of hydrogen-containing silicone oil and 8kg of water, then add 7kg of acetone and stir evenly to obtain the mixture; spray the mixture into 120kg of the second material in a stirring state, heat up to 86℃, mix evenly, and remove A...
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com