Antifungal paint for advertisements
An anti-mold and advertising technology, which is applied in paints containing biocide, anti-fouling/underwater coatings, luminous coatings, etc., can solve the problems of poor anti-mold performance and short service life, and achieve strong impact resistance and low production cost. The effect of low cost and simple production method
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] Weigh 27 parts by mass of phenolic resin, 15 parts by mass of polyamide, 7 parts by mass of toluene diisocyanate, 6 parts by mass of bentonite, 5 parts by mass of titanium dioxide, 4 parts by mass of nano-silica, 8 parts by mass of orthobutyl silicate, and 12 parts by mass of nitrile, 6 parts by mass of methyl methacrylate, 35 parts by mass of N, N dimethylacetamide, stirred for 50 minutes, mixed uniformly, then added 9 parts by mass of sodium lactate, and continued to stir for 30 minutes to obtain the anti-mold paint of the present invention .
Embodiment 2
[0014] Weigh 25 parts by mass of phenolic resin, 18 parts by mass of polyamide, 6 parts by mass of toluene diisocyanate, 7 parts by mass of bentonite, 4 parts by mass of titanium dioxide, 6 parts by mass of nano-silica, 9 parts by mass of orthobutyl silicate, propylene 11 parts by mass of nitrile, 7 parts by mass of methyl methacrylate, 30 parts by mass of N, N dimethylacetamide and stirred for 50 minutes, mixed uniformly, then added 9 parts by mass of sodium diacetate, and continued to stir for 30 minutes to obtain the anti-aging agent of the present invention. Mold paint.
Embodiment 3
[0016] Weigh 29 parts by mass of phenolic resin, 12 parts by mass of polyamide, 9 parts by mass of toluene diisocyanate, 5 parts by mass of bentonite, 6 parts by mass of titanium dioxide, 3 parts by mass of nano-silica, 5 parts by mass of orthobutyl silicate, and 13 parts by mass of nitrile, 4 parts by mass of methyl methacrylate, and 41 parts by mass of N,N dimethylacetamide, stirred for 50 minutes, mixed uniformly, then added 9 parts by mass of propyl p-hydroxybenzoate, and continued to stir for 30 minutes to obtain The anti-mold paint of the present invention.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com