Feed antibacterial agent containing copper-carrying X-type molecular sieve and preparation method of feed antibacterial agent
A molecular sieve and antibacterial agent technology, applied in the field of X-type molecular sieve copper-loaded feed antibacterial agent and its preparation, can solve problems such as large energy consumption, achieve the effects of low equipment requirements, reducing harm to humans and animals, and wide industrial value
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0053] Raw materials: Diatomite comes from the Liudaogou mining area in Linjiang, Jilin Province, and its main chemical composition and content are SiO 2 : 63.77%, Al 2 o 3 : 18.97%, Fe 2 o 3 : 1.48%, TiO 2 : 0.06%, CaO: 0.48%, K 2 O: 0.16%, Na 2 O: 0.04%. Aluminum hydroxide is analytically pure, white powder with the chemical formula Al(OH) 3 . Copper chloride dihydrate is analytically pure, green powder, chemical formula is CuCl 2 ·H 2 O.
[0054] The preparation process steps are as follows:
[0055] (1) Weigh 12.84g of sodium hydroxide and dissolve it in 115.6mL of distilled water, respectively take 10.07g of diatomite ore sample and 4.50g of aluminum hydroxide and join in the above-mentioned sodium hydroxide solution, and age with magnetic stirring for 30min to make Diatomaceous earth and aluminum hydroxide are fully dispersed in sodium hydroxide solution to form silica-alumina sol.
[0056] (2) Add the suspension obtained in step (1) into a 150.0 mL hydrothe...
Embodiment 2
[0060] The raw materials and steps are the same as in Example 1, except that 12.89g of sodium hydroxide is dissolved in 116.0mL of distilled water, and 10.83g of diatomite ore samples and 4.84g of aluminum hydroxide are added to the above-mentioned sodium hydroxide solution middle. Hydrothermal reaction at 110 ° C for 5h.
Embodiment 3
[0062] Same as the raw materials and steps in Example 1, the difference is: 13.20g sodium hydroxide is dissolved in 119.0mL distilled water, 5.17g of diatomite ore samples and 2.31g of aluminum hydroxide are added to the above-mentioned sodium hydroxide solution middle. Hydrothermal reaction at 110 ° C for 5h.
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com