Wood modifier, preparation method thereof, and method for modifying and treating wood with the modifier

A wood modification and modifier technology, applied in wood treatment, wood treatment details, wood impregnation, etc., can solve problems such as unfriendly human body and environment, and achieve the effects of strong loss resistance, easy realization and simple preparation process

Active Publication Date: 2020-11-27
NORTHWEST A & F UNIV
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Furthermore, in order to solve the technical defect that the existing wood preservative components are not friendly to the human body and the environment, the present invention adopts a plant natural component or a plant extract containing this natural component as an effective component to make wood improvement sex agent

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Wood modifier, preparation method thereof, and method for modifying and treating wood with the modifier
  • Wood modifier, preparation method thereof, and method for modifying and treating wood with the modifier
  • Wood modifier, preparation method thereof, and method for modifying and treating wood with the modifier

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0029] 1) Preparation of wood modifier

[0030] Put quercetin, catalyst and organic solvent into a reaction kettle respectively for mixing, and prepare uniformly at a temperature of 30-80° C. to obtain the wood modifier. The above components are in parts by weight, the parts by weight of the quercetin in the wood modifier is 1-10, the parts by weight of the catalyst in the wood modifier are 0.05-0.1, the organic The parts by weight of the solvent in the wood modifier are 200-1000. In the present embodiment, the parts by weight of quercetin is 1 part; the catalyst is potassium carbonate, and the parts by weight of potassium carbonate is 0.05 parts; the organic solvent is ethyl acetate, and the parts by weight of ethyl acetate is 200 parts, the above-mentioned combination Mix and prepare the reaction solution at 30°C to obtain the wood modifier.

[0031] 2) Wood modification treatment method

[0032]In this embodiment, the wood is modified by vacuum-pressurized impregnation t...

Embodiment 2

[0036] 1) Preparation of wood modifier

[0037] Put quercetin, catalyst and organic solvent into a reaction kettle respectively for mixing, and prepare uniformly at a temperature of 30-80° C. to obtain the wood modifier. The above components are in parts by weight, the parts by weight of the quercetin in the wood modifier is 1-10, the parts by weight of the catalyst in the wood modifier are 0.05-0.1, the organic The parts by weight of the solvent in the wood modifier are 200-1000. In the present embodiment, the parts by weight of quercetin is 10 parts; the catalyst is sodium carbonate, and the parts by weight of sodium carbonate is 0.1 parts; the organic solvent is pyridine, and the parts by weight of pyridine is 1000 parts, and the above components are Mixing and formulating into a reaction solution, the wood modifier is obtained.

[0038] 2) Wood modification treatment method

[0039] In this embodiment, the wood is modified by vacuum-pressurized impregnation treatment. ...

Embodiment 3

[0043] 1) Preparation of wood modifier

[0044] Put quercetin, catalyst and organic solvent into a reaction kettle respectively for mixing, and prepare uniformly at a temperature of 30-80° C. to obtain the wood modifier. The above components are in parts by weight, the parts by weight of the quercetin in the wood modifier is 1-10, the parts by weight of the catalyst in the wood modifier are 0.05-0.1, the organic The parts by weight of the solvent in the wood modifier are 200-1000. In the present embodiment, the parts by weight of quercetin are 5 parts; the catalyst is sodium hydroxide, and the parts by weight of sodium hydroxide is 0.1 parts; the organic solvent is N, N-dimethylformamide, N, N- The weight part of dimethylformamide is 800 parts, and the above components are mixed and prepared at 70° C. to form a reaction solution to obtain the wood modifier.

[0045] 2) Wood modification treatment method

[0046] In this embodiment, the wood is modified by vacuum-pressurized...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention belongs to the technical field of wood processing, and discloses a wood modifying agent capable of improving corrosion resistance of wood, a preparation method thereof and a method for modifying and treating wood through the modifying agent. The wood modifying agent comprises quercetin capable of improving the corrosion resistance of wood or natural flavone extract containing quercetin, and further comprises a catalyst and an organic solvent. The preparation method comprises the following steps: mixing quercetin or natural flavone extract containing quercetin, the catalyst and the organic solvent, and mixing uniformly at a temperature of 30-80 DEG C. After being modified by the wood modifying agent, free hydroxyl of wood generates chemical reaction with quercetin, so that thequercetin with corrosion resistance and bacteria inhibition is firmly combined inside the wood, and therefore, loss resistance is effectively improved, and corrosion resistance of wood is remarkablyimproved.

Description

technical field [0001] The invention belongs to the technical field of wood processing, and relates to a wood modifier capable of improving the corrosion resistance of wood, a preparation method of the wood modifier and a method for modifying and treating wood with the modifier. In particular, it relates to a wood modifier with quercetin or natural flavonoid extract containing quercetin as a component, a preparation method thereof and a method for modifying and treating wood with the wood modifier. Background technique [0002] Wood is a renewable and environment-friendly biomass material, which has the advantages of high strength-to-weight ratio, less energy consumption for processing, and relatively little environmental pollution. It plays a very important role in economic and social development and people's lives. However, because wood is composed of natural polymer compounds, there are deficiencies such as loose material, large variation in material properties, and vulne...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): B27K3/52B27K3/08B27K3/10B27K5/04
CPCB27K3/08B27K3/10B27K3/52B27K5/04
Inventor 闫丽雷亚芳杨芳霞上官蔚蔚毕振举方森苗
Owner NORTHWEST A & F UNIV