A water-based and ink-based technology, applied in inks, applications, household appliances, etc., can solve the problems of rising production costs of pearlescent inks and increasing prices of pearlescent pigments, and achieve increased versatility and practical quantification, enhanced pearlescent effects, and strong pearlescent effects Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] A water-based pearlescent medium suitable for PVC wallpaper printing ink, its raw material components are: 45% modified water-based polyurethane resin, 32% water, 0.2% aminomethyl propanol, and 1.5% defoamer , 5% hexylene glycol, 7% dipropylene glycol butyl ether, 5% slow drying agent, 2.6% surfactant, 0.3% alkali swelling thickener and 1.4% associative thickener;
[0026] The synthesis steps are as follows:
[0027] The first step: drop into modified water-based polyurethane resin, aminomethylpropanol and defoamer in the first stirring container, stirring speed 900rpm, stirring time is 20min, obtains the homogeneous mixture I of these each component;
[0028] The second step: put water (mass percentage 8%), dipropylene glycol butyl ether and hexylene glycol in the second stirring container, the stirring speed is 800rpm, and the stirring time is 20min to obtain the homogeneous mixture II of this component;
[0029] The third step: put the homogeneous mixture II obtaine...
Embodiment 2
[0033] A water-based pearlescent medium suitable for PVC wallpaper printing ink, its raw material components are: modified water-based polyurethane resin 40%, water 35%, aminomethyl propanol 0.3%, defoamer 1% , hexanediol 6%, dipropylene glycol butyl ether 8%, slow drying agent 4.5%, surfactant 2.8%, alkali swelling thickener 0.4% and associative thickener 2%;
[0034] The synthesis steps are as follows:
[0035] The first step: drop into modified water-based polyurethane resin, aminomethylpropanol and defoamer in the first stirring container, stirring speed 800rpm, stirring time is 20min, obtains the homogeneous mixture I of these each component;
[0036] The second step: put water (10% by mass), dipropylene glycol butyl ether and hexylene glycol into the second stirring container, the stirring speed is 900 rpm, and the stirring time is 20 min to obtain the homogeneous mixture II of this component;
[0037] The third step: put the homogeneous mixture II obtained in the secon...
Embodiment 3
[0041] A water-based pearlescent medium suitable for PVC wallpaper printing ink, its raw material components are: modified water-based polyurethane resin 47%, water 33%, aminomethyl propanol 0.1%, defoamer 1.2% , 4% hexylene glycol, 5% dipropylene glycol butyl ether, 6% slow drying agent, 2.5% surfactant, 0.2% alkali swelling thickener and 1% associative thickener;
[0042] The synthesis steps are as follows:
[0043] The first step: drop into modified water-based polyurethane resin, aminomethylpropanol and defoamer in the first stirring container, stirring speed 1000rpm, stirring time is 20min, obtains the homogeneous mixture I of these each component;
[0044] The second step: put water (9% by mass), dipropylene glycol butyl ether and hexylene glycol in the second stirring vessel, the stirring speed is 950rpm, and the stirring time is 20min to obtain the homogeneous mixture II of the components;
[0045]The third step: put the homogeneous mixture II obtained in the second s...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com