Antiskid and antibacterial protective boot and preparation method thereof
A technology for protective boots and antibacterial agents, which is applied in the fields of botanical equipment and methods, oxidative preparation of carboxylic acids, chemical instruments and methods, etc., can solve problems such as performance degradation of protective boots, cracks and separation of protective boots, etc. effect, increase in oxidation resistance, increase in service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0056] A kind of anti-slip antibacterial protective boots, made of the following raw materials in parts by weight: 100 parts of thermoplastic styrene-butadiene rubber, 2 parts of antibacterial agent, 1 part of antioxidant, 2 parts of diethyl phthalate, 1 part of paraffin wax, 1 part of stearic acid share;
[0057] The protective boots are prepared by the following steps:
[0058] Step S1: After heating the thermoplastic styrene-butadiene rubber at a temperature of 85° C., cutting the thermoplastic styrene-butadiene rubber into blocks;
[0059] Step S2: adding paraffin wax and stearic acid into a pulverizer for pulverization, passing through a 200-mesh sieve, and mixing to obtain a mixed powder;
[0060] Step S3: Mix the bulk thermoplastic styrene-butadiene rubber and the mixed powder prepared in step S1 at a temperature of 150°C for 30 minutes, then add antibacterial agents, antioxidants, and diethyl phthalate to continue Mixing 1h, obtained rubber material;
[0061] Step S...
Embodiment 2
[0074] A kind of anti-slip antibacterial protective boots, made of the following raw materials in parts by weight: 110 parts of thermoplastic styrene-butadiene rubber, 2.5 parts of antibacterial agent, 1.5 parts of antioxidant, 2.5 parts of diethyl phthalate, 3 parts of paraffin wax, 3 parts of stearic acid share;
[0075] The protective boots are prepared by the following steps:
[0076] Step S1: After heating the thermoplastic styrene-butadiene rubber at a temperature of 90° C., cutting the thermoplastic styrene-butadiene rubber into blocks;
[0077] Step S2: adding paraffin wax and stearic acid into a pulverizer for pulverization, passing through a 250-mesh sieve, and mixing to obtain a mixed powder;
[0078] Step S3: Mix the bulk thermoplastic styrene-butadiene rubber and the mixed powder prepared in step S1 at a temperature of 155°C for 35 minutes, then add antibacterial agents, antioxidants, and diethyl phthalate to continue Mixing 1.3h, obtained rubber material;
[0...
Embodiment 3
[0081] A kind of non-slip antibacterial protective boots, made of the following raw materials in parts by weight: 120 parts of thermoplastic styrene-butadiene rubber, 3 parts of antibacterial agent, 2 parts of antioxidant, 3 parts of diethyl phthalate, 5 parts of paraffin, 5 parts of stearic acid share;
[0082] The protective boots are prepared by the following steps:
[0083] Step S1: After heating the thermoplastic styrene-butadiene rubber at a temperature of 100° C., cutting the thermoplastic styrene-butadiene rubber into blocks;
[0084] Step S2: adding paraffin and stearic acid into a pulverizer for pulverization, passing through a 300-mesh sieve, and mixing to obtain a mixed powder;
[0085] Step S3: Mix the bulk thermoplastic styrene-butadiene rubber and the mixed powder prepared in step S1 at a temperature of 160°C for 40 minutes, then add antibacterial agents, antioxidants, and diethyl phthalate to continue Mixing 1.5h, obtained rubber material;
[0086] Step S4: ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com