Novel environment-friendly foam cement light soil and preparation method thereof
A foamed cement and lightweight soil technology, applied in the field of lightweight soil, can solve the problem of low strength of foamed cement lightweight soil, and achieve the effects of improving strength and toughness, improving shear strength and reducing agglomeration
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0049] A preparation method of a novel environmentally friendly foamed cement lightweight soil:
[0050] Stir and mix 0.05kg of toluene-2,6-diisocyanate and 6kg of tetrahydrofuran, then heat up to 50°C, add 1kg of banana stem fibers, continue to stir and mix for 2 hours, filter after stirring, collect the filtrate and put it in an oven, and use 65 Dry at ℃ for 1 h to obtain modified banana stem fibers.
[0051] 0.065kg of sodium lauryl sulfate, 0.01kg of cocamidopropyl betaine, 0.025kg of sodium carboxymethyl starch and 0.3kg of the first portion of water were stirred and mixed for 20min to obtain a foam mixture.
[0052] Stir and mix 0.19kg of modified banana stem fiber and 0.08kg of orange peel fiber for 10min, then add 1.5kg of slag and 8.5kg of cement, continue to stir for 2min, then add 4.7kg of the second portion of water, continue to stir for 1min, and then add the foam mixture , and continue to stir for 1 min to obtain a new type of environmentally friendly foamed cem...
Embodiment 2
[0054] A preparation method of a novel environmentally friendly foamed cement lightweight soil:
[0055] Stir and mix 0.14 kg of toluene-2,6-diisocyanate and 8 kg of tetrahydrofuran, then heat up to 60 ° C, add 1 kg of banana stem fibers, continue to stir and mix for 2 hours, filter after stirring, collect the filtrate and put it in an oven, and use 65 Dry at ℃ for 1 h to obtain modified banana stem fibers.
[0056] 0.09kg of sodium lauryl sulfate, 0.03kg of cocamidopropyl betaine, 0.06kg of sodium carboxymethyl starch and 0.3kg of the first portion of water were stirred and mixed for 20min to obtain a foam mixture.
[0057] Stir and mix 0.28kg of modified banana stem fiber and 0.14kg of orange peel fiber for 10min, then add 2.5kg of fly ash and 11kg of cement, continue to stir for 2min, add 6.2kg of the second part of water, continue to stir for 1min, and then add foam to mix liquid, and continue to stir for 1 min to obtain a new type of environmentally friendly foamed cemen...
Embodiment 3
[0059] A preparation method of a novel environmentally friendly foamed cement lightweight soil:
[0060] Stir and mix 0.1 kg of toluene-2,6-diisocyanate and 6 kg of tetrahydrofuran, then heat up to 55 ° C, add 1 kg of banana stem fibers, continue to stir and mix for 2 h, filter after stirring, collect the filtrate and put it in an oven, at 65 Dry at ℃ for 1 h to obtain modified banana stem fibers.
[0061] 0.09kg of sodium lauryl sulfate, 0.03kg of cocamidopropyl betaine, 0.06kg of sodium carboxymethyl starch and 0.3kg of the first portion of water were stirred and mixed for 20min to obtain a foam mixture.
[0062] Stir and mix 0.25kg of modified banana stem fiber and 0.12kg of orange peel fiber for 10min, then add 1.8kg of fly ash and 9.2kg of cement, continue to stir for 2min, then add 5.2kg of the second part of water, continue to stir for 1min, and then add foam The mixed solution was continuously stirred for 1 min to obtain a new type of environmentally friendly foamed c...