A chlorinated polyvinyl chloride, high-voltage power technology, which is applied to tubular articles, other household appliances, applications, etc., can solve the problems affecting the quality of buried pipeline works, road construction rolling, low strength and toughness, etc. Improved tensile yield strength and good mechanical properties
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] (1) Production casing:
[0038] (1) Ingredients: (by weight) chlorinated polyvinyl chloride resin powder: 100, nano-polyvinyl chloride resin: 8, heat stabilizer: 3, lubricant: 2, impact modifier: 8, processing modification Reactive agent: 2, flame retardant: 4, nano calcium carbonate: 3 mixed preparation;
[0039] (2) Stirring: Stir the prepared raw materials in a high-speed mixer until the temperature reaches 100-105°C, then stir in a low-speed cooling mixer to cool down to 60°C, and discharge for later use;
[0040] (3) sieve, use vibrating type sieve machine to sieve and reach 40 orders;
[0041] (4) Extrusion: Extrude the billet with a φ65 or φ55 twin-screw extruder, specifically using the German general temperature control method, that is, from the first area of the fuselage (185°C) to the confluence core (165°C), the temperature is constant Decrease, and then from the confluence core to the die, the operating temperature continues to rise (160-180°C);
[0042...
Embodiment 2
[0054] (1) Process steps for producing casing:
[0055] (1) Ingredients: (by weight) chlorinated polyvinyl chloride resin powder: 100, nano-polyvinyl chloride resin: 12, heat stabilizer: 3.5, lubricant: 3, impact modifier: 10, processing modification Reactive agent: 2.5, flame retardant: 3, nano calcium carbonate: 3 mixed preparation;
[0056] (2) Stirring: Stir the prepared raw materials in a high-speed mixer until the temperature reaches 100-105°C, then stir in a low-speed cooling mixer to cool down to 60°C, and discharge for later use;
[0057] (3) sieve, use vibrating type sieve machine to sieve and reach 40 orders;
[0058] (4) Extrusion: Extrude the billet with a φ65 or φ55 twin-screw extruder, specifically using the German general temperature control method, that is, from the first area of the fuselage (185°C) to the confluence core (165°C), the temperature is constant Decrease, and then from the confluence core to the die, the operating temperature continues to ris...