Rubber synchronous belt with safe polycyclic aromatic hydrocarbon content
A polycyclic aromatic hydrocarbon and synchronous belt technology, applied in the direction of transmission belts, V-belts, belts/chains/gears, etc., can solve the problems of difficult export, excessive PAHs content, non-compliance with EU environmental protection requirements, etc., to achieve low operating noise, transmission The effect of high speed and low shaft load
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] The following raw materials are weighed in parts by weight:
[0029] Neoprene PM-40 type 95 parts
[0030] Butadiene rubber BR9001 type 5 parts
[0031] Reinforcing agent 36 parts
[0032] Anti-aging agent 1.5 parts
[0033] Accelerator 0.3 parts
[0035] Magnesium oxide 4 parts
[0036] 1.4 parts of stearic acid
[0037] 5 parts of operating oil
[0038] Firstly, the belt colloid is formed through rubber masticating and mixing processes, and then the sheet is calendered, and the rubber synchronous belt of the present invention is obtained through steps such as molding, vulcanization, demoulding, back grinding, cutting, and inspection. Its multi-ring According to ZEK01-08 standard, the content of aromatic hydrocarbon PAHs was analyzed and detected by GC-MS method, and the result was 4.2ppm.
Embodiment 2
[0040] The following raw materials are weighed in parts by weight:
[0041] Neoprene PM-40 type 90 parts
[0042] Butadiene rubber BR9001 type 10 parts
[0043] Reinforcing agent 38 parts
[0044] Anti-aging agent 1.5 parts
[0045] Accelerator 0.3 parts
[0046] 3 parts zinc oxide
[0047] Magnesium oxide 2.4 parts
[0048] 1.4 parts of stearic acid
[0049] 7 parts of operating oil
[0050] Firstly, the belt colloid is formed through rubber masticating and mixing processes, and then the sheet is calendered, and the rubber synchronous belt of the present invention is obtained through steps such as molding, vulcanization, demoulding, back grinding, cutting, and inspection. Its multi-ring According to ZEK01-08 standard, the content of aromatic hydrocarbon PAHs was analyzed and detected by GC-MS method, and the result was 4.2ppm.
Embodiment 3
[0052] The following raw materials are weighed in parts by weight:
[0053] Neoprene PM-40 type 92 parts
[0054] Butadiene rubber BR9001 type 8 parts
[0055] Reinforcing agent 38 parts
[0056] Anti-aging agent 1.5 parts
[0057] Accelerator 0.3 parts
[0058] Zinc oxide 5 parts
[0059] Magnesium oxide 4 parts
[0060]1.5 parts of stearic acid
[0061] 6 parts of operating oil
[0062] Firstly, the belt colloid is formed through rubber masticating and mixing processes, and then the sheet is calendered, and the rubber synchronous belt of the present invention is obtained through steps such as molding, vulcanization, demoulding, back grinding, cutting, and inspection. Its multi-ring According to ZEK01-08 standard, the content of aromatic hydrocarbon PAHs was analyzed and detected by GC-MS method, and the result was 4.2ppm.