Air-entrapping sodium silicate perlite thermal insulation material
A thermal insulation material, sodium fume silicate technology, applied in the direction of climate sustainability, sustainable waste treatment, solid waste management, etc., can solve the problems of high hygroscopicity, poor thermal insulation effect, high strength, etc., to reduce exhaust emissions and save The effect of fuel resources
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0041] A gas-entrained sodium perlite insulation material, comprising the following formula:
[0042] Composition Weight ratio
[0043] water glass 1
[0044] Sodium fluorosilicate 0.15
[0045] Perlite 0.5
[0046] Red mud (quick hardening cement) 0.03
[0047] h 2 o 2 (hydrogen peroxide) 0.07
[0048] Polypropylene fiber 0.007
[0049] Hydroxypropyl methylcellulose 0.003
[0050] NNO (sodium methylene dinaphthalene sulfonate) 0.003.
[0051] The manufacturing process of the gas-entrained sodium silicate perlite insulation material comprises the following steps:
[0052] Step 1: Add sodium fluorosilicate as water glass curing agent into water glass under stirring, make it pre-react for 0.5-1.0 hours at room temperature, make sodium fluorosilicate hard agglomerate, at the same time add hypromell Base cellulose, NNO and polypropylene fibers are stirred, dissolved and dispersed in water glass to form a composite water glass coagulation liquid;
[0053] Step 2: At room...
Embodiment 2
[0056] A gas-entrained sodium perlite insulation material, comprising the following formula:
[0057] Composition Weight ratio
[0058] water glass 1
[0059] Sodium fluorosilicate 0.18
[0060] Perlite 0.8
[0061] Red mud (quick hardening cement) 0.03
[0062] h 2 o 2 (hydrogen peroxide) 0.09
[0063] Polypropylene fiber 0.007
[0064] Hydroxypropyl methylcellulose 0.003
[0065] NNO (sodium methylene dinaphthalene sulfonate) 0.003.
[0066] The manufacturing process of the gas-entrained sodium perlite insulation material is the same as that of the first embodiment above.
Embodiment 3
[0068] A gas-entrained sodium perlite insulation material, comprising the following formula:
[0069] Composition Weight ratio
[0070] water glass 1
[0071] Sodium fluorosilicate 0.16
[0072] Perlite 0.7
[0073] Red mud (quick hardening cement) 0.03
[0074] h 2 o 2 (hydrogen peroxide) 0.08
[0075] Polypropylene fiber 0.007
[0076] Hydroxypropyl methylcellulose 0.003
[0077] NNO (sodium methylene dinaphthalene sulfonate) 0.003.
[0078] The manufacturing process of the gas-entrained sodium perlite insulation material is the same as that of the first embodiment above.
PUM