Method for preparation of dimethyl ether
A catalyst and dimethyl ether technology, which is applied in the field of preparation of dimethyl ether catalysts, can solve the problems of low catalyst performance, high reaction temperature, and inability to meet industrial production, and achieve high activity, stability, and high activity effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] 2% lanthanum nitrate (purchased from Tianjin Damao Chemical Reagent Factory) aqueous solution 200g and 200g gamma-alumina (Dalian Ruike Technology Co., Ltd.) powder were kneaded and extruded, then roasted at 550°C for 5 hours, cooled, and pulverized to The lanthanum oxide accounts for 1% of the modified γ-alumina for use below 100 mesh. Add 150g of water into the colloid mill (purchased from Dalian Xinghuo Packaging Machinery Factory, model is JM-50), start the colloid mill, then add the above-mentioned modified γ-alumina 30g, grind for 4 hours, and take the methanol synthesis catalyst component ( Dalian Ruike Technology Co., Ltd.) 60g (on a dry basis), aluminum glue (Dalian Ruike Technology Co., Ltd.) 3g (on a dry basis) were added to the colloid mill, and continued to grind for 2 hours; wherein the methanol synthesis catalyst group It is the intermediate product carbonate mixture of copper-zinc-aluminum methanol synthesis catalyst, which contains basic copper carbonat...
Embodiment 2
[0022] The method and steps of catalyst preparation are as in Example 1, except that 1% lanthanum nitrate and 1% cerium nitrate (purchased from Tianjin Damao Chemical Reagent Factory) mixed aqueous solution is used to knead gamma-alumina, the grinding time is 8 hours, and the colloid The particle size of each component in the method is below 3 microns, and the dimethyl ether catalyst is obtained by drying, roasting and pulverizing as well. The ratio of methanol synthesis catalyst component to methanol dehydration catalyst component is 2:1, and the specific surface area of the prepared catalyst is 158.45m 2 / g, the pore volume is 0.3528cc / g, and the catalyst activity evaluation results are shown in Table 2.
Embodiment 3
[0024] The method and steps of catalyst preparation are as in Example 2. After adding modified gamma-alumina, the grinding time is 8 hours, and 150 g (in dry basis) of the intermediate colloidal carbonate mixture of copper-zinc-aluminum methanol synthesis catalyst is added, The substance contains basic copper carbonate, basic zinc carbonate and aluminum oxide, and after roasting at 500°C, the weight contents of copper oxide, zinc oxide and aluminum oxide are 55.43%, 24.63% and 8.84% respectively. After grinding, it is measured that the particle size of each component in the colloid is below 3 microns, and the dimethyl ether catalyst is also obtained by drying, roasting and pulverizing. The ratio of the methanol synthesis catalyst component to the methanol dehydration catalyst component is 5:1, and the catalyst activity evaluation results are shown in Table 3.
PUM
Property | Measurement | Unit |
---|---|---|
specific surface area | aaaaa | aaaaa |
specific surface area | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com