A wood and degreasing tank technology, which is applied in wood treatment, wood processing equipment, wood treatment details, etc., can solve the problems of great variation and difficulty in the permeability of degreasing liquid, and it is difficult to accurately reflect the penetrating characteristics of degreasing liquid of large-scale test pieces, etc. , to achieve the effect of low production cost, convenient operation and easy realization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of wood degreasing method, adopts following steps:
[0019] (1) Preparation of color retention solution: according to the mass ratio m 连二亚硫酸钠 :m 氯化钠 =10:0.1, uniformly mix sodium dithionite and sodium chloride, and then prepare an aqueous solution with a concentration of 0.5% by mass percentage to prepare a color-preserving solution;
[0020] (2), canning: according to the volume ratio V 木材 / V 保色液 =1:0.5 color retention liquid and wood are packed into high-pressure degreasing tank; wherein wood refers to pine sawn timber;
[0021] (3) Color retention treatment: keep warm for 7 hours at a temperature of 20°C and a pressure of 0.9 MPa, and then drain the liquid; after draining the liquid, open the degreasing tank and unload the color retention wood;
[0022] (4) Dry the color-preserving wood in the flue gas at 50°C for 3 days, then continue to dry in the flue gas at 80°C for 3 days, and then continue to dry in the flue gas at 95°C for 1 day to obtain degreased ...
Embodiment 2
[0024] A kind of wood degreasing method, adopts following steps:
[0025] (1) Preparation of color retention solution: according to the mass ratio m 连二亚硫酸钠 :m 氯化钠 =10:1, uniformly mix sodium dithionite and sodium chloride, then prepare an aqueous solution with a mass percentage concentration of 2.5%, and prepare a color-preserving solution;
[0026] (2), canning: according to the volume ratio V 木材 / V 保色液 =1:1.0 color retention liquid and wood are packed into high-pressure degreasing tank; wherein wood refers to pine sawn timber;
[0027] (3) Color retention treatment: keep warm for 6 hours at a temperature of 30°C and a pressure of 0.6 MPa, and then drain the liquid; after draining the liquid, open the degreasing tank and unload the color retention wood;
[0028] (4) Dry the color-preserving wood in flue gas at 55°C for 3 days, continue to dry in flue gas at 85°C for 2 days, and then continue to dry in flue gas at 100°C for 0.5 days to obtain degreased wood; The gas is th...
Embodiment 3
[0030] A kind of wood degreasing method, adopts following steps:
[0031] (1) Preparation of color retention solution: according to the mass ratio m 连二亚硫酸钠 :m 氯化钠 =10:2, uniformly mix sodium dithionite and sodium chloride, then prepare an aqueous solution with a mass percentage concentration of 3.5%, and prepare a color-preserving solution;
[0032] (2), canning: according to the volume ratio V 木材 / V 保色液 =1:0.5 color retention liquid and timber are packed into high-pressure degreasing tank; Wherein timber refers to Chinese fir sawn timber;
[0033] (3) Color retention treatment: keep warm for 5 hours at a temperature of 40°C and a pressure of 0.4 MPa, and then drain the liquid; after draining the liquid, open the degreasing tank and unload the color retention wood;
[0034] (4) Dry the color-preserving wood in flue gas at 50°C for 3 days, then continue to dry in flue gas at 90°C for 2 days, and then continue to dry in flue gas at 95°C for 1 day to obtain degreased wood; T...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com