Ink-jet oil painting canvas and manufacturing method thereof
An oil canvas and inkjet technology, applied in the direction of coating, etc., can solve the problems of poor pertinence and applicability, and less inkjet canvas, and achieve the effects of high applicability, good color fastness, and good color expression
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
specific Embodiment 1
[0023] A kind of ink-jet oil canvas disclosed by the present invention, described oil canvas is followed by base material, base coat and surface coat from bottom to top, and its specific preparation method is:
[0024] a. Select polyester fabric as the base material and put it in the oven, and dry it at 80°C for 5 minutes;
[0025] b. Evenly coat the undercoat on the substrate after drying and setting, dry at 100°C, and repeat the same drying once more. The composition of the undercoat is 35 parts of kaolin, 1 part of polyvinyl alcohol 1799 , 1 part of polyvinyl alcohol 1788 type, 30 parts of adhesive, 0.5 part of auxiliary agent, 1 part of water;
[0026] c. On the semi-finished oil canvas coated with the base coat in step b, evenly coat the top coat and put it into an oven, and dry it at 105°C for 5 minutes, wherein the top coat consists of 10 parts of silicon dioxide, polyvinyl alcohol 1799 type 1 1 part, 1 part of polyvinyl alcohol 1788 type, 30 parts of special adhesi...
specific Embodiment 2
[0028] A kind of ink-jet oil canvas disclosed by the present invention, described oil canvas is followed by base material, base coat and top coat from bottom to top, and its specific preparation method is:
[0029] a. Select pure cotton fabric as the base material and put it in the oven, and dry it at 90°C for 6 minutes;
[0030] b. Evenly coat the undercoat on the substrate after drying and setting, dry at 110°C, and repeat the same drying once more. The composition of the undercoat is 40 parts of talcum powder, polyvinyl alcohol 1799 type 1 Parts, 2 parts of polyvinyl alcohol 1788 type, 35 parts of adhesive, 1 part of auxiliary agent, 15 parts of water;
[0031] c. On the semi-finished oil canvas coated with the base coat in step b, evenly coat the top coat and put it into an oven, and dry it at 110°C for 6 minutes, wherein the top coat consists of 13 parts of silicon dioxide, polyvinyl alcohol 1799 type 1 1 part, 1 part of polyvinyl alcohol 1788 type, 35 parts of specia...
specific Embodiment 3
[0033] This embodiment is an existing non-flame-retardant ink-jet oil canvas, and the oil canvas is sequentially composed of a base material, a primer layer and an ink-absorbing coating layer from bottom to top, and its specific production method is as follows:
[0034] a. Select the polyester-cotton blended fabric as the base material and put it in the oven, and dry it at 100°C for 7 minutes;
[0035] b. Evenly coat the undercoat on the base material after drying and setting, dry at 120 ° C, and repeat the same drying once again, wherein the composition of the undercoat is 20 parts of kaolin, 25 parts of lithopone, poly 1 part of vinyl alcohol 1799 type, 1 part of polyvinyl alcohol 1788 type, 40 parts of adhesive, 2 parts of auxiliary agent, 30 parts of water;
[0036] c. On the semi-finished oil canvas coated with the base coat in step b, evenly coat the top coat and put it into an oven, and dry it at 115°C for 7 minutes, wherein the top coat consists of 15 parts of silic...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com