Layered energy-saving and environmental-protection honeycomb briquette
An energy-saving, environmentally friendly, honeycomb coal technology, applied in the energy field, can solve the problems of unable to maintain the original shape, short combustion time, incomplete combustion, etc., and achieve the effect of saving coal energy, sufficient combustion, and good combustion connection.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] (1) Weigh 500kg of crushed crop straw charcoal powder, 200kg of cinder and 0.4kg of combustion enhancer, mix, add 10kg of water, mix well, and set aside;
[0034] (2) Weigh 600kg of pulverized coal cinder, 600kg of coal and 0.4kg of sulfur fixation agent to mix, add 18kg of water, mix well, and set aside;
[0035] (3) Weigh 450kg of pulverized coal and 450kg of clay, 1-3kg of combustion accelerant, and 1-3kg of sulfur-fixing agent, add 15kg of water, mix well, and set aside;
[0036] (4) Add part of (1) the obtained mixture to the mould, and properly extrude to the lowermost line of the mould, to obtain the fifth layer of briquette;
[0037] (5) According to the method described in (4), sequentially extrude to obtain the fourth, third, second, and first layers;
[0038] ⑹Naturally air-dry.
Embodiment 2
[0040] (1) Weigh 500t of crushed crop straw charcoal powder, 200t of cinder and 0.8t of combustion enhancer, mix, add 12t of water, mix well, and set aside;
[0041] (2) Weigh 600t of pulverized coal cinder, 600t of coal and 0.8t of sulfur fixative to mix, add 20t of water, mix well, and set aside;
[0042] (3) Weigh 450t of crushed coal, 450t of clay, 2t of combustion accelerant, 2t of sulfur-fixing agent, add 32t of water, mix well, and set aside;
[0043] (4) Add part of (1) the obtained mixture to the mould, and properly extrude to the lowermost line of the mould, to obtain the fifth layer of briquette;
[0044] (5) According to the method described in (4), sequentially extrude to obtain the fourth, third, second, and first layers;
[0045] ⑹ Just dry.
Embodiment 3
[0047] (1) Weigh 500 catties of crushed crop straw charcoal powder, 200 catties of cinder and 1 catties of combustion aid, mix, add 14 catties of water, mix well, and set aside;
[0048] (2) Weigh 600 jin of pulverized cinder, 600 jin of coal and 1 jin of sulfur-fixing agent to mix, add 24 jin of water, mix well, and set aside;
[0049] (3) Weigh 450 jin of coal and 450 jin of clay after crushing, 3 jin of combustion enhancer, 3 jin of sulfur-fixing agent, add 36 jin of water, mix well, and set aside;
[0050] (4) Add part of (1) the obtained mixture to the mould, and properly extrude to the lowermost line of the mould, to obtain the fifth layer of briquette;
[0051] (5) According to the method described in (4), sequentially extrude to obtain the fourth, third, second, and first layers;
[0052] ⑹ Just dry.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com