Slurry disperse dye and preparation method and appliance
A technology for disperse dyes and liquid disperse dyes, applied in the field of slurry disperse dyes and their preparation, can solve the problems of small water consumption, short printing process, large waste water discharge, etc. The effect of poor fastness and low sewage discharge
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0058] 18.0g butyl acrylate, 2.5g acrylonitrile, 0.5g acrylic acid, 0.5g N-methylolacrylamide, 0.2g pentaerythritol tetraacrylate, 1.0g ethylene glycol dimethacrylate, 2.0g isotridecyl Acrylic ester, 0.5g emulsifier SP-80, 1.0g sodium dodecylsulfonate, 0.5g isomeric tridecyl alcohol polyoxyethylene ether (12) and 60.5g water were mixed, and fully stirred to form an emulsion. Dissolve 1.0 g of ammonium persulfate in 11.8 g of water at room temperature and stir well to form an initiator solution. Take half of the mass of the emulsion and half of the mass of the initiator solution and put them into the reaction device, stir while heating, and raise the temperature to 70°C. When the temperature reaches 70°C, under stirring state, slowly add the mixture of half of the mass of the remaining emulsion and the mass of the initiator solution dropwise at the same time, and the dropping time is 120 minutes. After the dropwise addition, the stirring was continued for 120 min at 74°C±2°C t...
Embodiment 2
[0060] Mix 12.0g of the original dye (2), 0.6g of isomeric tridecyl alcohol polyoxyethylene ether (8) potassium salt of phosphate, 0.6g of stearic acid polyoxyethylene ether (9), and 86.8g of water in a sand mill Medium grinding until the particle size of the dye is 1-3 μm, to prepare 100 g of liquid disperse dye. Add 0.02g of H90 synthetic thickener and 2.0g of functional prepolymer A to the liquid disperse dye, and stir thoroughly to obtain slurry-like disperse dye A.
Embodiment 3
[0062] Mix 15.0g of the original dye (4), 1.0g of potassium tridecyl alcohol ether (6) phosphate ester, 2.0g of tridecyl alcohol polyoxyethylene ether (12), and 82.0g of water in sand Grinding in a grinding device until the particle size of the dye is 1-3 μm, and 100 g of liquid disperse dye is obtained. Add 0.02g of H90 synthetic thickener and 1.5g of functional prepolymer A to the above liquid disperse dye, and stir thoroughly to obtain slurry-like disperse dye B.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
length | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com