A technology of anti-slip rubber and composition, applied in application, shoe sole, clothing and other directions, can solve the problems of poor storage stability of neoprene raw rubber, increased Mooney viscosity, poor storage stability, etc., and achieves expansion of effective temperature range, The effect of improving the anti-skid performance and the anti-skid performance of the ice surface
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] In this embodiment 1, the ice surface dynamic anti-skid rubber is composed of the following components by weight:
[0044] Neoprene 15 parts
[0045] Solution polystyrene butadiene rubber T2100 15 parts
[0046] Carboxylated nitrile rubber X740 55 parts
[0047] White carbon black 12 parts
[0048] 12 parts waste rubber powder
[0049] Antiager 1010 1 part
[0050] Polyethylene glycol PEG4000 2 parts
[0051] Silane coupling agent Si69 2 parts
[0052] Polyethylene wax 2 parts
[0054] Sulfur 2.5 parts
[0055] Vulcanization accelerator D 1 part
[0056] Vulcanization accelerator DM 1 part.
[0057] All the rubber materials except zinc oxide, sulfur, and vulcanization accelerators are put into the banbury mixer for internal mixing, deglue at 105°C, and stand at room temperature for 24 hours, then knead on the double-roller open mill, and add accurately weighed oxide Zinc, sulfur, and vulcanization accelerator are mixed evenly, and ...
Embodiment 2
[0061] In this embodiment 2, the composition and production method of the dynamic anti-slip rubber on the ice surface are basically the same as the production method in embodiment 1, except that 20 parts of solution-polymerized styrene-butadiene rubber, 15 parts of white carbon black, and 15 parts of waste rubber powder share.
[0062] The anti-slip rubber product on ice prepared above has an anti-slip coefficient of 0.42 and 0.43 on the front palm on the frosty ice surface, 0.39 and 0.40 on the heel on the dry ice surface, and 0.39 and 0.40 on the heel on the wet ice surface. 0.32 followed by 0.32.
Embodiment 3
[0064] In this embodiment 3, the composition of dynamic anti-slip rubber on the ice surface, the production method are basically the same as the production method in embodiment 1, except that 50 parts of carboxylated nitrile rubber, 10 parts of white carbon black, and 10 parts of waste rubber powder share.
[0065] The anti-slip rubber product on ice surface prepared above has an anti-slip coefficient of 0.35 on the front palm and 0.34 on the heel on the frosty ice surface, 0.30 on the front palm and 0.30 on the heel on the dry ice surface, and 0.30 on the front palm on the wet ice surface. 0.28 followed by 0.29.