Alkali slag water-retaining agent and preparation method and application thereof
A technology of water-retaining agent and alkali slag, which is applied in the field of alkali-slag water-retaining agent and its preparation, to achieve the effects of convenient use, alleviating environmental pollution problems, and low production energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] 1) Mix the alkali residue and water uniformly to obtain a mixture of alkali residue and water. The mixture of alkali residue and water is dehydrated. After dehydration, the moisture content is 96%, and the chloride ion content is 1.3wt% of the total solid mass in the mixture. Of chlor-alkali residue;
[0029] 2) Drying the chlor-alkali slag with the chloride ion content of 1.3 wt% of the total solid mass in the mixture to obtain the chlor-alkali slag;
[0030] 3) After mixing the prepared chlor-alkali slag and granulated blast furnace slag powder at a ratio of 80wt%:20wt%, they are added to a ball mill and pulverized to a 0.30mm sieve residue of 9wt% mixed powder to obtain alkali Slag water retention agent.
Embodiment 2
[0032] 1) After mixing the alkali residue and water uniformly, a mixture of alkali residue and water is obtained. The mixture of alkali residue and water is dehydrated. After dehydration, the water content is 94%, and the chloride ion content is 0.9wt% of the total solid mass in the mixture. Of chlor-alkali residue;
[0033] 2) Drying the chlor-alkali slag with the chloride ion content of 0.9 wt% of the total solid mass in the mixture to obtain the chlor-alkali slag;
[0034] 3) After mixing the prepared chlorinated alkali slag and limestone powder at a ratio of 60wt%:40wt%, they are added to a ball mill and pulverized to a mixed powder with a 0.30mm sieve residue of 7wt% to obtain an alkali slag water retaining agent .
Embodiment 3
[0036] 1) After mixing the alkali residue and water uniformly, a mixture of alkali residue and water is obtained. The mixture of alkali residue and water is dehydrated. After dehydration, the moisture content is 95%, and the chloride ion content is 0.5wt% of the total solid mass in the mixture. Of chlor-alkali residue;
[0037] 2) Drying the chlor-alkali slag with the chloride ion content of 0.5 wt% of the total solid mass in the mixture to obtain the chlor-alkali slag;
[0038] 3) The prepared chlor-alkali slag and fly ash are mixed uniformly in the ratio of 70wt%: 30wt%, then added to the ball mill, pulverized to a 0.30mm sieve residue of 6wt% mixed powder, to obtain the alkali slag water retention Agent.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com