Environment-friendly wallpaper and preparation method thereof
A wallpaper and environmental protection technology, applied in paper, papermaking, paper coating, etc., can solve the problems of wallpaper endangering human life and health, poor air permeability, and damp walls
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] (1) 32 parts by weight of acetone, 6 parts by weight of sodium hexametaphosphate, 5 parts by weight of polyvinyl chloride with a weight average molecular weight of 81,000, 12 parts by weight of melamine-formaldehyde resin, 40 parts by weight of acrylic resin, 2 parts by weight of Silicon carbide, 6 parts by weight of polydimethylsiloxane and 10 parts by weight of bamboo charcoal powder with a particle diameter of 200nm are mixed to obtain a waterproof coating;
[0019] (2) Heat the paper at an initial temperature of 20°C for 3 minutes at a heating rate of 2°C / min to perform the first preheating treatment; then raise the temperature at a heating rate of 7°C / min for 2 minutes to perform the second preheating treatment;
[0020] (3) Apply the waterproof paint on the preheated paper, heat it at 110°C for 35 minutes, and emboss it to make the environmentally friendly wallpaper A1.
Embodiment 2
[0022] (1) 50 parts by weight of acetone, 9 parts by weight of sodium pyrophosphate, 15 parts by weight of polyvinyl chloride with a weight average molecular weight of 88,000, 18 parts by weight of melamine-formaldehyde resin, 50 parts by weight of acrylic resin, 5 parts by weight of carbonized Silicon, 9 parts by weight of emulsified silicone oil and 10 parts by weight of bamboo charcoal powder with a particle diameter of 300nm are mixed to make a waterproof coating;
[0023] (2) Raise the temperature of the paper at an initial temperature of 25°C for 5 minutes at a heating rate of 5°C / min to perform the first preheating treatment; then raise the temperature at a heating rate of 10°C / min for 5 minutes to perform the second preheating treatment;
[0024] (3) Apply the waterproof paint on the preheated paper, heat it at 130°C for 50 minutes, and emboss it to make the environmental wallpaper A2.
Embodiment 3
[0026] (1) 40 parts by weight of acetone, 8 parts by weight of sodium lauryl sulfate, 10 parts by weight of polyvinyl chloride with a weight average molecular weight of 85,000, 15 parts by weight of melamine-formaldehyde resin, 45 parts by weight of acrylic resin, 3 parts by weight Parts by weight of silicon carbide, 7 parts by weight of polyoxypropylene glyceryl ether and 10 parts by weight of bamboo charcoal powder with a particle diameter of 250nm are mixed to obtain a waterproof coating;
[0027] (2) Heat the paper at an initial temperature of 23°C for 3 minutes at a heating rate of 3°C / min to perform the first preheating treatment; then raise the temperature at a heating rate of 8°C / min for 3 minutes to perform the second preheating treatment;
[0028] (3) Apply the waterproof paint on the preheated paper, heat it at 120°C for 40 minutes, and emboss it to make the environmental wallpaper A3.
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com