Drying method for wood
A wood drying and wood technology, which is applied in the field of agriculture and forestry, can solve the problems of poor product quality stability, deformed paint adhesion, wood quality decline, etc., and achieve the effect of benefiting corrosion resistance, reducing warping deformation, increasing vibration and evaporation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A kind of wood drying method, comprises the following steps:
[0037] A. Pre-plan the wood, and cut the wood into boards of the same size; among them, the wood is cut to a thickness of 22mm.
[0038] B. Soak the pre-planed wood in saturated salt water for 1 day.
[0039] C. Wrap the wood soaked in salt water with tinfoil and bake it; wherein, the baking temperature is 170°C; the baking time is 1 hour.
[0040] D. smear the wood anti-cracking agent with the baked wood, then carry out microwave and ultrasonic drying; Wherein, described wood anti-cracking agent comprises the mixture of turpentine and camphor, by weight, 75 parts of turpentine, 25 parts of camphor. The control conditions of microwave and ultrasonic drying are: the power of ultrasonic is 1KW, and the frequency is 20KHz; the power of microwave is 1KW, and the frequency is 1000MHz. The drying environment is: absolute pressure 0.02MPa, dry bulb temperature 70°C, wet bulb temperature 8°C; drying time 1 hour. ...
Embodiment 2
[0049]A kind of wood drying method, comprises the following steps:
[0050] A. Pre-plan the wood, and cut the wood into boards of the same size; among them, the wood is cut to a thickness of 30mm.
[0051] B. Soak the pre-planed wood in saturated salt water for 1 day.
[0052] C. Apply wood anti-cracking agent to the wood soaked in salt water, then wrap it in tin foil and bake it. Wherein, the baking temperature is 250° C.; the baking time is 0.5 hour. Wherein, the wood anti-cracking agent comprises a mixture of turpentine and camphor, by weight, 60 parts of turpentine and 40 parts of camphor.
[0053] D. apply wood anti-cracking agent to the baked wood, then carry out microwave and ultrasonic drying; Wherein, described wood anti-cracking agent comprises the mixture of turpentine and camphor, by weight, 60 parts of turpentine, 40 parts of camphor. The control conditions of microwave and ultrasonic drying are: the power of ultrasonic is 3KW, and the frequency is 28KHz; the p...
Embodiment 3
[0063] A kind of wood drying method, comprises the following steps:
[0064] A. Pre-plan the wood, and cut the wood into boards of the same size; among them, the wood is cut to a thickness of 28mm.
[0065] B. Soak the pre-planed wood in saturated salt water for 1 day.
[0066] C. Apply wood anti-cracking agent to the wood soaked in salt water, then wrap it in tin foil and bake it. Wherein, the baking temperature is 200° C.; the baking time is 0.7 hours. Wherein, the wood anti-cracking agent comprises a mixture of turpentine and camphor, by weight, 80 parts of turpentine and 20 parts of camphor.
[0067] D. apply wood anti-cracking agent to the baked wood, then carry out microwave and ultrasonic drying; Wherein, described wood anti-cracking agent comprises the mixture of turpentine and camphor, by weight, 80 parts of turpentine, 20 parts of camphor. The control conditions of microwave and ultrasonic drying are: the power of ultrasonic is 2KW, and the frequency is 25KHz; the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com