A technology of complexes and macromolecules, applied in chemical instruments and methods, luminescent materials, etc., can solve problems such as poor luminescence performance and insufficient coordination number of rare earth ions, and achieve good luminescence performance, simple preparation process, and good luminescence performance Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] A preparation method of a warm white macromolecular complex fluorescent powder containing europium and terbium zinc, comprising the following steps:
[0028] 1) Preparation of polymer ligands
[0029] Weigh 0.4414g of 4-vinylbenzoic acid, 3.19mL of methyl methacrylate, and 0.0035g of initiator azobisisobutyronitrile, and dissolve them in dimethyl sulfoxide solvent, and ultrasonically shake them to fully dissolve , and then transfer the solution to a test tube with a support, and fix it in a constant temperature water bath, seal the test tube opening with a rubber stopper with a glass catheter, the branch of the test tube is open, and insert the glass catheter into the bottom of the test tube , nitrogen deoxygenation at room temperature through the glass catheter for at least 30 minutes; after the nitrogen deoxygenation is completed, connect the branch of the test tube with the glass catheter port and seal it with a rubber tube; raise the temperature of the constant temp...
Embodiment 2
[0041] A preparation method of a warm white macromolecular complex fluorescent powder containing europium and terbium zinc, comprising the following steps:
[0042] 1) Preparation of polymer ligands
[0043] Weigh 0.4413g of 4-vinylbenzoic acid, 3.18mL of methyl methacrylate, and 0.0037g of initiator azobisisobutyronitrile, dissolve them in dimethyl sulfoxide solvent, and ultrasonically shake them to fully dissolve , and then transfer the solution to a test tube with a support, and fix it in a constant temperature water bath, seal the test tube opening with a rubber stopper with a glass catheter, the branch of the test tube is open, and insert the glass catheter into the bottom of the test tube , nitrogen deoxygenation at room temperature through the glass catheter for at least 30 minutes; after the nitrogen deoxygenation is completed, connect the branch of the test tube with the glass catheter port and seal it with a rubber tube; raise the temperature of the constant temperat...
Embodiment 3
[0055] A preparation method of a warm white macromolecular complex fluorescent powder containing europium and terbium zinc, comprising the following steps:
[0056] 1) Preparation of polymer ligands
[0057] Weigh 0.4415g of 4-vinylbenzoic acid, 3.17mL of methyl methacrylate, and 0.0036g of initiator azobisisobutyronitrile, and dissolve them in dimethyl sulfoxide solvent, and ultrasonically shake them to fully dissolve , and then transfer the solution to a test tube with a support, and fix it in a constant temperature water bath, seal the test tube opening with a rubber stopper with a glass catheter, the branch of the test tube is open, and insert the glass catheter into the bottom of the test tube , nitrogen deoxygenation at room temperature through the glass catheter for at least 30 minutes; after the nitrogen deoxygenation is completed, connect the branch of the test tube with the glass catheter port and seal it with a rubber tube; raise the temperature of the constant temp...