Pegmatite-type spodumene flotation collecting agent and preparation method and application thereof
A collector and pegmatite technology, applied in the field of pegmatite-type spodumene flotation collector and its preparation, can solve the problems of collectors such as poor adaptability to temperature, poor selectivity of agents, and poor solubility of agents , to achieve the effects of stable production technical indicators, strong water solubility at low temperature, and reduced dosage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0046] The pegmatite type spodumene flotation collector of the present embodiment is mainly made of the following components in parts by weight: 50 parts of petroleum sulfonate, 45 parts of coconut oil fatty acid diethanolamide and 5 parts of lauric acid share.
[0047] The preparation method of above-mentioned pegmatite type spodumene flotation collector comprises the steps:
[0048] (1) First add 15 parts of water into the mixing tank, turn on the stirring function, then slowly add sodium laurate into it, and stir for 30-60 minutes until it is completely dissolved;
[0049] (2) Add petroleum sulfonate and coconut oil fatty acid diethanolamide to the material obtained in step (1) in proportion, stir for 60-90min, make it fully mixed, and obtain pegmatite type spodumene flotation Receiver.
Embodiment 2
[0051] The pegmatite type spodumene flotation collector of the present embodiment is mainly made of the following components in parts by weight: 75 parts of petroleum sulfonate, 15 parts of coconut oil fatty acid diethanolamide and sodium laurate 10 servings.
[0052] The preparation method of above-mentioned pegmatite type spodumene flotation collector comprises the steps:
[0053] (1) First add 30 parts of water into the mixing tank, turn on the stirring function, then slowly add sodium laurate into it, and stir for 30-60 minutes until it is completely dissolved;
[0054] (2) Add petroleum sulfonate and coconut oil fatty acid diethanolamide to the material obtained in step (1) in proportion, stir for 60-90min, make it fully mixed, and obtain pegmatite type spodumene flotation Receiver.
Embodiment 3
[0056] The pegmatite type spodumene flotation collector of the present embodiment is mainly made of the following components in parts by weight: 65 parts of petroleum sulfonate, 35 parts of coconut oil fatty acid diethanolamide and sodium laurate 10 servings.
[0057] The preparation method of above-mentioned pegmatite type spodumene flotation collector comprises the steps:
[0058] (1) First add 30 parts of water into the mixing tank, turn on the stirring function, then slowly add sodium laurate into it, and stir for 30-60 minutes until it is completely dissolved;
[0059] (2) Add petroleum sulfonate and coconut oil fatty acid diethanolamide to the material obtained in step (1) in proportion, stir for 60-90min, make it fully mixed, and obtain pegmatite type spodumene flotation Receiver.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com