A kind of environment-friendly organometallic corrosion inhibitor and its preparation method and application
An environment-friendly, organometallic technology, applied in the field of environment-friendly organometallic corrosion inhibitor and its preparation, metal corrosion inhibitor and its preparation field, can solve the problems of dependence on imports, difficult circulation of medium, unfriendly environment, etc. The effect of solving instability, excellent corrosion inhibition performance and good corrosion inhibition effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] Embodiment 1: Preparation of 100kg organic carboxylic acid additive premixed sample S1
[0036] Because several kinds of organic carboxylic acids are solid, and no chemical reaction occurs after mixing with each other, it is purely physical mixing, so it is only necessary to accurately weigh the following raw materials according to the quantity and stir them well:
[0037] p-nitrobenzoic acid 32kg
[0038] Isononanoic acid 22kg
[0039] Sebacic acid 46kg
[0040] The mixed sample S1 is used for subsequent corrosion inhibitor preparation.
Embodiment 2
[0041] Embodiment 2: Preparation of 100kg organic carboxylic acid additive premixed sample S2
[0042] According to the method described in Example 1, mix according to the following ratio:
[0043] m-iodophenyl acid 12kg
[0044] Benzoic acid 26kg
[0045] Isononanoic acid 11kg
[0046] Sebacic acid 51kg
[0047] The mixed sample S2 is used for subsequent corrosion inhibitor preparation.
Embodiment 3
[0048] Embodiment 3: Preparation of 1000kg environment-friendly organometallic corrosion inhibitor sample S3
[0049] Add 535kg of purified water into the open 1500L reactor with stirring, start stirring, and add the following materials to the reactor in turn:
[0050] Benzotriazole 70kg
[0051] Sodium Gluconate 120kg
[0053] S1 90kg
[0054] Pyrazine 80kg
[0055] Sodium glutamate 50kg
[0056] Sodium hydroxide 8kg
[0057] After adding all the materials, stir for 0.5h to 1h until all the materials are dissolved and mixed evenly to obtain a homogeneous transparent liquid. Finally, add 2kg of sodium hydroxide, stir to dissolve and mix evenly. The pH value of the test solution is between 11-12, which meets the requirements , filtering, filling.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com