An anti-rust oil and a new type of technology are applied in the preparation of new-type anti-rust oil and the field of new-type anti-rust oil, which can solve the problems of low leveling and uniformity, reducing the anti-rust performance of anti-rust oil and affecting the anti-rust effect, etc. Achieve the effect of improving leveling and uniformity, improving corrosion inhibition and enhancing rust prevention effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] A new type of anti-rust oil, comprising the following raw materials in parts by weight: 70 parts of machine oil, 8 parts of composite corrosion inhibitor, 5 parts of sodium hydroxide, 2 parts of paraffin, 20 parts of diluent, 20 parts of butyl cellulose, propylene glycol butyl 1 part ether, 1 part butyl hydroxyanisole.
[0033] The composite corrosion inhibitor consists of 12 parts by weight of N,N-laurylamine, 3 parts of dodecyl succinic acid, and 6 parts of polyoxyethylene alkyl ether acid phosphate.
[0034] A kind of preparation method of novel antirust oil, comprises the following steps
[0035] S1 Preparation of composite corrosion inhibitor: select quantitative N, N-laurylamine, dodecyl succinic acid and polyoxyethylene alkyl ether acid phosphate to add to the container, heat the temperature to 90°C, and stir for 10 minutes to prepare a composite corrosion inhibitor. etchant;
[0036] S2 Mixing of raw materials: Pour mechanical oil into the reaction kettle, hea...
Embodiment 2
[0042] A new antirust oil, comprising the following raw materials in parts by weight: 75 parts of kerosene, 10 parts of composite corrosion inhibitor, 7 parts of sodium hydroxide, 4 parts of paraffin, 30 parts of thinner, 30 parts of butyl cellulose, propylene glycol methyl ether 3 parts of acetate, 1 part of dibutyl hydroxytoluene.
[0043] The composite corrosion inhibitor consists of 15 parts by weight of N,N-laurylamine, 4 parts of dodecyl succinic acid, and 9 parts of polyoxyethylene alkyl ether acid phosphate.
[0044] A kind of preparation method of novel antirust oil, comprises the following steps
[0045] S1 Preparation of composite corrosion inhibitor: select quantitative N,N-laurylamine, dodecyl succinic acid and polyoxyethylene alkyl ether acid phosphate into the container, heat the temperature to 95°C, and stir for 9 minutes to prepare a composite corrosion inhibitor. etchant;
[0046] S2 Mixing of raw materials: Pour kerosene into the reaction kettle, heat and ...
Embodiment 3
[0052] A new antirust oil, comprising the following raw materials in parts by weight: 80 parts of machine oil, 12 parts of composite corrosion inhibitor, 6 parts of sodium carbonate, 3 parts of paraffin, 25 parts of thinner, 25 parts of butyl cellulose, ethylene glycol 2 parts, 2 parts of tert-butyl hydroquinone.
[0053] The composite corrosion inhibitor consists of 18 parts by weight of N,N-laurylamine, 4 parts of dodecyl succinic acid, and 8 parts of polyoxyethylene alkyl ether acid phosphate.
[0054] A kind of preparation method of novel antirust oil, comprises the following steps
[0055] S1 Preparation of composite corrosion inhibitor: select quantitative N,N-laurylamine, dodecyl succinic acid and polyoxyethylene alkyl ether acid phosphate into the container, heat the temperature to 95°C, and stir for 9 minutes to prepare a composite corrosion inhibitor. etchant;
[0056] S2 Mixing of raw materials: Pour mechanical oil into the reaction kettle, heat and stir until the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com