A technology of masking paper and adhesives, applied in the direction of adhesives, adhesive types, ester copolymer adhesives, etc., can solve the problems of harmfulness to the human body, residual glue, and non-environmental protection of masking paper adhesives, and achieve high adhesion force effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Example Embodiment
[0051] Example 1
[0052] The formula used to prepare masking paper adhesive is as follows:
[0053] Isooctyl acrylate 150
[0054] Butyl acrylate 15
[0055] Methyl methacrylate 50
[0056] Hydroxyethyl acrylate 3
[0057] acrylic acid 3
[0058] NMA 4
[0059] Water 235
[0060] Sodium bicarbonate 0.1
[0061] 710 alcohol ether phosphate 2.9
[0062] Ammonium persulfate 0.6.
[0063] The preparation method is as follows:
[0064] S100. Preparation of pre-emulsion monomer: In the first reactor, add 80% of the 710 alcohol ether phosphate and 30% of the water in the formula, mix and stir, then add all the isooctyl acrylate and acrylic acid in the formula Butyl ester, methyl methacrylate, hydroxyethyl acrylate and acrylic acid, stir well;
[0065] S200. In the second reactor, add 45% of the water in the formula, the remaining 710 alcohol ether phosphate and all th...
Example Embodiment
[0070] Example 2
[0071] The formula used to prepare masking paper adhesive is as follows:
[0072] Isooctyl acrylate 165
[0073] Butyl acrylate 10
[0074] Methyl methacrylate 42
[0075] Hydroxyethyl acrylate 5
[0076] acrylic acid 2
[0077] NMA 5
[0078] Water 265
[0079] Sodium bicarbonate 0.3
[0080] 710 alcohol ether phosphate 1.8
[0081] Ammonium persulfate 0.97
[0082] The preparation method is as follows:
[0083] S100. Preparation of pre-emulsion monomer: In the first reactor, add 90% of the 710 alcohol ether phosphate and 45% of the water in the formula, mix and stir, then add all the isooctyl acrylate and acrylic acid in the formula Butyl ester, methyl methacrylate, hydroxyethyl acrylate and acrylic acid, stir well;
[0084] S200. In the second reactor, add 40% of the water in the formula, the remaining 710 alcohol ether phosphate and all th...
Example Embodiment
[0089] Example 3
[0090] The formula used to prepare masking paper adhesive is as follows:
[0091] Isooctyl acrylate 189
[0092] Butyl acrylate 8
[0093] Methyl methacrylate 56
[0094] Hydroxyethyl acrylate 7
[0095] acrylic acid 4
[0096] NMA 7
[0097] Water 249
[0098] Sodium bicarbonate 0.4
[0099] 710 alcohol ether phosphate 1
[0100] Ammonium persulfate 1.25
[0101] The preparation method is as follows:
[0102] S100. Preparation of pre-emulsion monomer: In the first reactor, add 85% of the 710 alcohol ether phosphate and 40% of the water in the formula, mix and stir evenly, then add all the isooctyl acrylate and acrylic acid in the formula Butyl ester, methyl methacrylate, hydroxyethyl acrylate and acrylic acid, stir well;
[0103] S200. In the second reactor, add 30% of the water in the formula, the remaining 710 alcohol ether phosphate and a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap