Flotation separation method of antimony sulfide gold minerals

A mineral flotation and separation technology, applied in flotation, solid separation, etc., can solve the problems of affecting gold recovery rate, waste of resources, difficult separation, etc., and achieve the effect of less chemical consumption, simple process and less energy consumption

Active Publication Date: 2013-03-27
白银金锑矿业科技有限公司
View PDF3 Cites 21 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002] In some sulfide ores of gold-bearing minerals such as pyrite or arsenopyrite, there are often associated antimony sulfide minerals with an antimony grade of 0.3% to 1%. It is difficult to separate in the flotation process. Generally, some antimony concentrates are obtained after hand-selected antimony nuggets, and the rest are directly flotation with gold-lo

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Flotation separation method of antimony sulfide gold minerals
  • Flotation separation method of antimony sulfide gold minerals
  • Flotation separation method of antimony sulfide gold minerals

Examples

Experimental program
Comparison scheme
Effect test

Example Embodiment

[0014] Example 1

[0015] 1. Mineral raw materials:

[0016] The antimony content in the mineral raw materials used is 0.37%, and the gold is 1.86 g / ton. The phase analysis shows that the antimony-bearing minerals are mainly antimonite, and the gold-bearing minerals are pyrite and arsenopyrite.

[0017] 2. The total dosage of flotation reagent is:

[0018]

[0019] The operating steps and technical conditions are as follows:

[0020] In the mixed flotation process, the ore is added to the ore grinder to grind until the mineral monomers are dissociated. Under natural pH conditions, lead nitrate is added as the activator of antimony gold minerals, and then butyl xanthate is added for collection Agent, add 2 at the end # No. oil is used as a foaming agent for mixed flotation to obtain a mixed antimony gold concentrate; in the process of flotation separation, activated carbon is used for demedication, then sodium hydroxide is used to adjust the pH to 8.5, and then sodium humate and starch ...

Example Embodiment

[0021] Example 2

[0022] 1. Mineral raw materials:

[0023] The antimony content in the mineral raw materials used is 0.62%, and the gold is 2.15 g / ton. The phase analysis shows that the antimony-bearing minerals are mainly antimonite, and the gold-bearing minerals are pyrite and arsenopyrite.

[0024] 2. The total dosage of flotation reagent is:

[0025]

[0026] The operating steps and technical conditions are as follows:

[0027] In the mixed flotation process, the ore is added to the ore grinder to grind until the mineral monomers are dissociated. Under natural pH conditions, lead nitrate is added as the activator of antimony gold minerals, and then butyl xanthate is added for collection Agent, add 2 at the end # No. oil is used as a foaming agent for mixed flotation to obtain a mixed antimony gold concentrate; in the process of flotation separation, activated carbon is used to demedicate, then sodium hydroxide is used to adjust the pH to 9, and then sodium humate and starch are u...

Example Embodiment

[0028] Example 3

[0029] 1. Mineral raw materials:

[0030] The antimony content in the mineral raw materials used is 0.87%, and the gold is 3.26 g / ton. The phase analysis shows that the antimony-bearing minerals are mainly antimonite, and the gold-bearing minerals are pyrite and arsenopyrite.

[0031] 2. The total dosage of flotation reagent is:

[0032]

[0033] The operating steps and technical conditions are as follows:

[0034] In the mixed flotation process, the ore is added to the ore grinder to grind until the mineral monomers are dissociated. Under natural pH conditions, lead nitrate is added as the activator of antimony gold minerals, and then butyl xanthate is added for collection Agent, add 2 at the end # No. oil is used as a foaming agent for mixed flotation to obtain a mixed antimony gold concentrate; in the process of flotation separation, use activated carbon to remove the drug, and then adjust the pH to 9.5 with sodium hydroxide, and then use sodium humate and starch ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

A flotation separation method of antimony sulfide gold minerals comprises the steps of performing bulk flotation to obtain antimony-gold mixed concentrate firstly and then separating the antimony-gold mixed concentrate to obtain antimony concentrate and gold concentrate, wherein in the bulk flotation, lead nitrate is taken as an activator for the antimony gold minerals, while sodium n-butylxanthate is used as a collecting agent and 2# oil is taken as a foaming agent; and in the flotation separation process, active carbon is used for reagent removal, while sodium hydroxide is used for adjusting the pH value to be 8.5-9.5, sodium humate and starch are used as a gold-containing mineral inhibitor and N, N-sodium diethyldithiocarbamate is used as the antimony mineral collecting agent. According to the flotation separation method, the antimony sulfide minerals can be effectively separated from the gold-carrying minerals through flotation, so that the antimony concentrate having the antimony grade of 33.82%-37.28% and the recovery rate of 87.21%-91.62% is obtained, and simultaneously, the gold concentrate having the grade of 40.27-45.81g/ton and the recovery rate of 85.64%-92.16% is obtained, through bulk flotation and further separation under the conditions that the feeding antimony grade is 0.37%-0.87% and the gold grade is 1.86-3.26 g/ton.

Description

1. Technical field [0001] The invention relates to a mineral flotation separation method, in particular to an antimony gold sulfide mineral flotation separation method. 2. Background technology [0002] In some sulfide ores of gold-bearing minerals such as pyrite or arsenopyrite, there are often associated antimony sulfide minerals with an antimony grade of 0.3% to 1%. It is difficult to separate in the flotation process. Generally, some antimony concentrates are obtained after hand-selected antimony nuggets, and the rest are directly flotation with gold-loaded pyrite and arsenopyrite to contain impurities in gold concentrates, and antimony is used as the gold smelting process Harmful elements, if the content of antimony is too high, it will not only increase the cost of gold smelting, but also affect the recovery rate of gold, which will not only increase the economic burden of the enterprise but also waste resources. 3. Contents of the invention [0003] The object of t...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): B03D1/00
Inventor 魏宗武钟景裕谢尚文
Owner 白银金锑矿业科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products