Water-based imitated marble multi-color paint and preparation and construction method thereof
A technique of imitating marble and colorful paint, applied in the field of paint, can solve the problems of unsightly appearance of the overall floor, difficulty in keeping the color consistent, and color difference of dry-hanging marble, etc., to achieve a solemn and solemn decorative effect, keep the painting beautiful, and rich in texture.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] The method for making water-based imitation marble colorful paint, comprises the following steps,
[0037] (1) Weigh 200 parts of deionized water by weight, add 3.5 parts of hydroxyethyl cellulose, and stir at 700 rpm for 30 minutes;
[0038] (2) Weigh and add 5.5 parts of multifunctional additives, 0.5 parts of wetting agent, 1.5 parts of defoamer, 8.5 parts of ethylene glycol, 17.5 parts of film-forming aids, and stir at 700 rpm for 15 minutes;
[0039] (3) Weigh and add 5.5 parts of polyurethane thickener, 450 parts of silicone acrylic emulsion, 2.5 parts of alkali swelling thickener, 2.5 parts of leveling agent, 2.0 parts of anti-settling agent, 2.0 parts of preservative, 700 rpm / min stirring for 30 minutes;
[0040] (4) Weigh and add 200 parts of colored rock chips, and stir at 600 rpm for 10 minutes.
[0041] The leveling agent is mixed with organic modified silicone leveling agent and fluorocarbon modified polyacrylic acid ammonium salt leveling agent in a ra...
Embodiment 2
[0043] The method for making water-based imitation marble colorful paint, comprises the following steps,
[0044] (1) Weigh 300 parts of deionized water by weight, add 5.5 parts of hydroxyethyl cellulose, and stir at 900 rpm for 30 minutes;
[0045] (2) Weigh and add 3.5 parts of multifunctional additives, 2.0 parts of wetting agent, 2.5 parts of defoamer, 10.5 parts of ethylene glycol, 20.5 parts of film-forming aids, and stir at 900 rpm for 15 minutes;
[0046] (3) Weigh and add 2.5 parts of polyurethane thickener, 350 parts of silicone acrylic emulsion, 4.5 parts of alkali swelling thickener, 4.5 parts of leveling agent, 3.0 parts of anti-settling agent, 3.0 parts of preservative, 700 rpm / min stirring for 30 minutes;
[0047] (4) Weigh and add 300 parts of colored rock chips, and stir at 600 rpm for 10 minutes.
[0048] The leveling agent is mixed with organic modified silicone leveling agent and fluorocarbon modified polyacrylic acid ammonium salt leveling agent in a rat...
Embodiment 3
[0050] The method for making water-based imitation marble colorful paint, comprises the following steps,
[0051] (1) Weigh 250 parts of deionized water by weight, add 5.0 parts of hydroxyethyl cellulose, and stir at 900 rpm for 30 minutes;
[0052] (2) Weigh and add 4.5 parts of multifunctional additives, 1.5 parts of wetting agent, 2.0 parts of defoamer, 10.0 parts of ethylene glycol, 20.0 parts of film-forming aid, and stir at 900 rpm for 15 minutes;
[0053] (3) Weigh and add 3.5 parts of polyurethane thickener, 400 parts of silicone acrylic emulsion, 3.0 parts of alkali swelling thickener, 3.0 parts of leveling agent, 2.5 parts of anti-settling agent, 2.5 parts of preservative, 900 rpm / min stirring for 30 minutes;
[0054] (4) Weigh and add 250 parts of colored rock chips, and stir at 600 rpm for 10 minutes.
[0055] The leveling agent is mixed with organic modified silicone leveling agent and fluorocarbon modified polyacrylic acid ammonium salt leveling agent in a ra...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com