A technology of copper selenite and zinc selenite, applied in application, chemical instruments and methods, inorganic chemistry and other directions, can solve the problems of difficult to control product quality, large fluctuation of selenium content, difficult preparation and operation, etc., to achieve saving The effect of preparation time, slowing down the reaction rate, and improving process efficiency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] Embodiment 1: the preparation method of zinc selenite
[0044] A preparation method of zinc selenite of the present invention, comprises the following steps:
[0045] Start stirring, and the purity is that 98% selenium dioxide 583g joins in the beaker that 1000g water is housed, and then adding purity is 98% basic zinc chloride 532g, after basic zinc chloride dissolves, add 168g sodium bicarbonate, And adjust the pH value to 5.0 with 5% sodium bicarbonate solution, and stir to make it fully react for 1 h. Then filter, wash, dry in an oven, and pulverize to obtain 902.4 g of zinc selenite product.
[0046] Through detection and analysis, Zn in the zinc selenite product that present embodiment obtains 2+ The content is 33.2%, the total selenium content is 40.2%, and the water loss rate of the product at 105°C is 0.56%, that is, Zn 2+ : Se 4+ =1:1, the yield is 94% (calculated as zinc), and the purity is 98%.
[0047] Among them, total selenium is detected by atomic f...
Embodiment 2
[0048] Embodiment 2: the preparation method of zinc selenite
[0049] A preparation method of zinc selenite of the present invention, comprises the following steps:
[0050] Turn on the stirring, and add 532.8Kg of selenium dioxide with a purity of 98% to a 5m tank with 390Kg of water 3 In the reaction kettle, add 458Kg of basic zinc sulfate with a purity of 98% to the reaction system, add 168Kg sodium bicarbonate after the basic zinc sulfate dissolves, and adjust the pH value to 5.5 with 5% sodium bicarbonate solution, stir to make it fully Reaction 1.5h. Then filter, wash, oven dry, pulverize, obtain zinc selenite product 745Kg.
[0051] Through detection and analysis, Zn in the zinc selenite that present embodiment obtains 2+ The content is 33.1%, the total selenium content is 40.2%, and the water loss rate of the product at 105°C is 0.72%, that is, Zn 2+ : Se 4+ =1:1, the yield is 97% (calculated as zinc), and the purity is 98%.
Embodiment 3
[0052] Embodiment 3: the preparation method of copper selenite
[0053] A preparation method of copper selenite of the present invention, comprises the following steps:
[0054] Turn on the stirring, and add 244.2Kg of selenium dioxide with a purity of 98% to a 5m tank with 336Kg of water 3 In the reaction kettle, add 213.5Kg basic copper chloride with a purity of 98% to the reaction system, add 84Kg potassium bicarbonate after the basic copper chloride dissolves, and adjust the pH value with a mass concentration of 5% potassium hydrogencarbonate solution 8.0, stirred to make it fully react for 2h, then centrifuged, the wet material was washed, dried, and pulverized to obtain 366Kg of copper selenite product. The basic copper chloride is selected from dry tailings or unqualified graded materials in the preparation of feed grade basic copper chloride products.
[0055] Through detection and analysis, Cu in the copper selenite obtained in the present embodiment 2+ The content...