A fiber reinforced concrete and ultra-high-strength steel technology, applied in the field of building materials, can solve the problems of low viscosity and strength not reaching the C120 strength level, and achieve the effects of low viscosity, optimized mixing ratio, and improved crack resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] The ultra-high pumping ultra-high-strength steel fiber concrete prepared in this embodiment, the raw material ratio (1m 3 Concrete material consumption) as shown in Table 1:
[0029]Table 1: C150 ultra-high-strength steel fiber reinforced concrete mix design (kg / m 3 )
[0030] cement
microbeads
mineral powder
steel fiber
mixing water
450
300
120
130
550
760
80
150
20
[0031] Step 1: Mix and stir river sand and basalt particles evenly for 30 seconds to obtain a mixture;
[0032] Step 2: mix the mixture obtained in step 1 with cement, mineral admixtures, and 80% mixing water for 60 seconds, and stir evenly; the weight of the cement is 34.35% of the aggregate weight, and the mineral admixture The weight of material is 41.98% of aggregate weight, and the weight of described 80% mixing water is 9.16% of aggregate weight; Described aggrega...
Embodiment 2
[0040] The ultra-high pumping ultra-high-strength steel fiber concrete prepared in this embodiment, the raw material ratio (1m 3 Concrete material consumption) as shown in Table 3:
[0041] Table 3: C150 ultra-high-strength steel fiber reinforced concrete mix design (kg / m 3 )
[0042] cement
microbeads
mineral powder
steel fiber
mixing water
500
200
220
80
660
660
120
150
22
[0043] Step 1: Mix and stir river sand and basalt particles evenly for 30 seconds to obtain a mixture;
[0044] Step 2: Mix the mixture obtained in step 1 with cement, mineral admixtures, and 80% mixing water for 60 seconds, and stir evenly; the weight of the cement is 37.88% of the aggregate weight, and the mineral admixture The weight of material is 37.88% of aggregate weight, and the weight of described 80% mixing water is 9.09% of aggregate weight; Described aggreg...
Embodiment 3
[0052] The ultra-high pumping ultra-high-strength steel fiber concrete prepared in this embodiment, the raw material ratio (1m 3 Concrete material consumption) as shown in Table 5:
[0053] Table 5: C150 ultra-high-strength steel fiber reinforced concrete mix design (kg / m 3 )
[0054] cement
microbeads
mineral powder
river sand
steel fiber
mixing water
580
200
170
50
600
680
140
150
21
[0055] Step 1: Mix and stir river sand and basalt particles evenly for 30 seconds to obtain a mixture;
[0056] Step 2: mix the mixture obtained in step 1 with cement, mineral admixtures, and 80% mixing water for 60 seconds, and stir evenly; the weight of the cement is 45.31% of the aggregate weight, and the mineral admixture The weight of material is 32.81% of aggregate weight, and the weight of described 80% mixing water is 9.38% of aggregate weight; Described aggreg...
PUM
Property | Measurement | Unit |
---|---|---|
specific surface area | aaaaa | aaaaa |
specific surface area | aaaaa | aaaaa |
specific surface area | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com