A technology for the production of sodium antimonate and antimony oxide, applied in chemical instruments and methods, antimonate/antimonite, inorganic chemistry, etc., can solve the problems of unsatisfactory raw material utilization and conversion rate, and achieve saving raw material consumption , improve the conversion rate, and promote the effect of conversion
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for producing sodium antimonate with antimony oxide, the production steps are:
[0019] (1) Heat the raw material antimony oxide at 300°C for 20 minutes under the condition of feeding air, then add it into the reaction vessel, add 25% hydrochloric acid and water into the reaction vessel, the addition amount is 1000g Add 250ml of hydrochloric acid and 500ml of water to the antimony raw material, stir at a speed of 250 rpm, add sodium polyacrylate during the stirring, and the amount of sodium polyacrylate added is 1% of the weight of the antimony oxide raw material;
[0020] (2) Add sodium hydroxide to the reaction vessel, the amount added is 40% of the weight of the antimony oxide raw material, continue to stir and control the reaction temperature to 50°C, after 40 minutes of reaction, feed oxygen into the reaction vessel to make the reaction mixture Under the oxygen pressure of 0.2MPa;
[0021] (3) Slowly add hydrogen peroxide into the reaction vessel. The tot...
Embodiment 2
[0024] A method for producing sodium antimonate with antimony oxide, the production steps are:
[0025] (1) Heat the raw material antimony oxide at 320°C for 20 minutes under the condition of feeding air, then add it into the reaction vessel, add 25% hydrochloric acid and water into the reaction vessel, the addition amount is 1000g oxidation Add 250ml of hydrochloric acid and 500ml of water to the antimony raw material, stir at a speed of 250 rpm, add sodium polyacrylate during the stirring, and the amount of sodium polyacrylate added is 2% of the weight of the antimony oxide raw material;
[0026] (2) Add sodium hydroxide to the reaction vessel, the amount added is 45% of the weight of the antimony oxide raw material, continue to stir and control the reaction temperature to 60°C, and after 30 minutes of reaction, feed oxygen into the reaction vessel to make the reaction mixture Under the oxygen pressure of 0.2MPa;
[0027] (3) Slowly add hydrogen peroxide into the reaction v...
Embodiment 3
[0030] A method for producing sodium antimonate with antimony oxide, the production steps are:
[0031] (1) Heat the raw material antimony oxide at 310°C for 20 minutes under the condition of feeding air, then add it into the reaction vessel, add 25% hydrochloric acid and water into the reaction vessel, the addition amount is 1000g Add 250ml of hydrochloric acid and 500ml of water to the antimony raw material, stir at a speed of 250 rpm, add sodium polyacrylate during the stirring, and the amount of sodium polyacrylate added is 1.5% of the weight of the antimony oxide raw material;
[0032] (2) Add sodium hydroxide to the reaction vessel in an amount of 42% of the weight of the antimony oxide raw material, continue to stir and control the reaction temperature to 55°C, and after 35 minutes of reaction, inject oxygen into the reaction vessel to make the reaction mixture Under the oxygen pressure of 0.2MPa;
[0033] (3) Slowly add hydrogen peroxide into the reaction vessel. The ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com